O1 hardness

Patrick Chase

O1 gets to be really brittle above Rc60 or so. I personally agree with George's oft-stated opinion that its sweet spot for non-laminated edge tools is closer to Rc59, and that Hock's Rc62 O1 plane irons are far too brittle. Even 60-61 sounds a little high to me

With that said, it depends on the application. Chisels require higher toughness than planes, both because they tend to be used at lower edge angles (for BD planes at least) and because we chop with them. An Rc62 O1 chisel would be basically useless, whereas I expect a Hock O1 iron would work perfectly well at 32 or 35 deg.

Laminated tools are a completely different matter of course. A softer backend both directly helps with impact loads, and allows you to do some other things via forging to tolerate higher hardness in the bit.

Re: Pictures of Various Honing Options

#27

Re: Thanks!

david weaver

Yes on the imanishi. I've had a bunch of those. Actually, I've had one of everything you said there.

I think that Naniwa had the snow white before the choseras, but I don't know the history that well. All three of their main lines were around when I started buying. I never went backwards into the more primitive stuff like the omura and lobster (but I have bought large coarse stones, just didn't like any of them that much because they are either too porous and hard or too soft).

I didn't like the arashiyama/takenoko 6k stone, but it would've been decent for knives.

(i'm going to go all over the place, my mind is disorganized this afternoon - it always is, but the turbo disorganized button must've been pushed by someone else).

I think the thing with naniwa, speculating, is that they found themselves in high end knife shops in japan and they created a progression that is just about the most ideal that I've seen for doing a knife with a bright polish cosmetic goal. The choseras are dreamy if you can keep them in continuous use, they're uniform and fast cutting. the 10k stops shy of super fineness, but that kind of super fineness is not useful sharpening knives - the 10k was chosen deliberately, I'm sure, and it's about perfect.

Before the choseras, my understanding is that the snow white was a low cost and extremely popular stone (for good reason).

When all is said and done, I agree, most of the modern stuff is a bit more user friendly than the old stuff. I think the old stuff was made hard to retain flatness because there would be more pro users who were used to learning a stone and who would be more annoyed by flattening. We've flip flopped that and switched it around.

825 frictionite is still my dream hone for feel, but they're only about the size of a shapton and probably $250 if you could find one. The feel is divine, but the shapton is probably more practical, same with the chosera. If one finds an unused 825 (I got one from george, and eventually sold it - I just didn't think I wanted to waste it sharpening tools, and razors don't need honing that often - it was designed to be a bench stone for razor factories according to the literature attached to it), it's probably borderline sin to waste one at this point. The lady who baked the frictionite stones is long gone and I don't think anyone has had luck duplicating it. The market would be small, anyway.

re: the naturals. $500 or so is probably the upper end of cost in utility. That's about what it costs to get a really lovely type 30 suita that is fine and hard. I have a short fat one, as well as a type 24 shiro, and ...well, i have a whole bunch of others, but the ones typical of what you could find are those. the seller I referred to selling ohira mine stuff, and some shobu and others, got $230 for the 1.8kg stubby ohira stone that I used above. nicer shape, it's probably in the 400-500 range.

I don't want to offend anyone, but I probably will. I have been through about $30K of japanese natural stones now (I sell them to undercut dealers who are not honest), and the stones that get well above $500 are either collector stones - and I can't debate their collector value - or just as often, they are overpromised and oversold stones that should be cheaper.

Or they're sold to people without discussion of things like color and its effect of fineness. Kiita japanese stones are seen as extremely desirable, but they usually aren't finer. I will get a buyer from time to time who sends me a message that they have a $1500 kiita stone and a white suita that I just flipped at cost (perhaps $400) and that the suita is better. They're offended.

My point being, if you do ever get into natural stones, send me a message. I won't sell anyone on here anything - i'm not trying to make money - but I can help you find reasonable natural stones on buyee that would let you get a taste. Decent swipes at tomae stones that are a bit undersized can be had for $100 or so. Suita, just above that. The bigger stones aren't necessarily better, they're just bigger and the market pays for shape, color, attributes and size.

I'd advise staying away from most other naturals (agates, etc.), because they really aren't practical. Same with la lune and other rare birds from europe. they're not that great. Add coticules to the list- capable, but variable and bad capability for the price.

Idwall from the UK are nice, but not always easy to find and you have to like a trans ark (that's what they're similar to) to appreciate them. Charnley - same, except they are variable. Some are soft, some harder, some coarser, some finer. They can border on being mildy friable and softer feeling, which is undesirable.

Hone slates - stay away, especially for woodworking. If they're any good (water of ayr, escher, etc) they've gotten way overpriced.

Re: Pictures of Various Honing Options

#28

Re: O1 hardness

david weaver

I think 60 is OK, but I'm guessing. There could be other confounding factors.

AI says their chisels are 61, and they do quite well. If they're actually 61, I don't know, but they're close to that (I've had chisels tested on a versitron before, and have a good idea of what numbers in plainer steels feel like between 53 and 61)

I've had monstrously hard O1 irons that have done OK before, too (knight had an iron that I believe was cryo treated. It was HARD for O1, but did better than hock's irons. I had two of them, and they were both the same (the knights). I've also had irons that are usually good (eskilstuna, bergs) that are very chippy. I think I might put them in the oven. I know they're not harder than knight's irons.

I wasn't surprised to see beach's page showing Steve Knight's irons holding up quite well. I'm going to go look after posting this, but am guessing that Hock's had a significant gap.

One other aside, stubai's chisels are also specified at 61 IIRC, and they're similar feeling to the AI chisels on an oilstone. Not sure, but they might have more other stuff - I don't follow what the current carving tool makers put in their tools (like pfeil), just suspect that it's not as plain as O1, but in both cases (stubai and pfeil), it's surprisingly good.

Re: Pictures of Various Honing Options

#29

Pfeil

Wiley Horne--So. Calif.

Hi David,

I like Pfeil carving tools also. Here is info from the Pfeil site,

“All pfeil tools are sharpened and honed, ready to use.

Chrome vanadium steel, special alloy made to pfeil specifications, combines outstanding elasticity with unsurpassed edge-holding properties.

We forge all our own tools.

Tools are hardened to edge of bevel. Blades electronically hardened to exacting tolerances. Tempered to HRC 59-61, depending on purpose of tool.”

Wiley

Re: Pictures of Various Honing Options

#30

Re: Pfeil

david weaver

Thanks, Wiley. someone had told me before that they were chrome vanadium, but I didn't want to quote it because I'd never read it from the source.

A friend got the pfeil chisels long ago before they had their shorter more american-style chisels. I just remember that they sharpened really easily and were very fine. Pfeil does a good job.

My older marples parers are sort of like that, too. On the back, they proudly stamped (in ink, fortunately, not stamped into the steel) "chrome vanadium". When I got them, I thought, Oh Jeez...boxwood handles, nice proportions, and.....chrome vanadium? I was prepared for them to be gummy, but they're quite nice.

I like pfeil carving tools as much as vintage (some of that may be bias because they're not half worn out when you find them), I just wish there was somewhere to get them other than woodcraft - in the US, that is. Not for any reason other than Woodcraft and now Japan Woodworker's very hefty standard markups. (not asking anyone else to agree with that, just stating it).

Across the board, there are examples like, kitayama stone on stand $37 in japan, low $60s from certain retailers in the US, $105 from Japan woodworker.

Re: Pictures of Various Honing Options

#31

Hardness and cryo treatment

Patrick Chase

Good point about hardness and refrigeration (a.k.a. "cryo treatment").

Converting any retained austenite to martensite vi refrigeration will certainly improve the achievable toughness at any given hardness (or vice-versa), so it would tend to allow higher hardness in any given application.

I still think that Rc 61-62 in a non-laminated tool is pushing it a bit for O-1 though. To be honest I wouldn't be surprised if the AI's were a little softer than billed, and that's not necessarily a bad thing.

Every tool (and every user) is different though, so what really matters are the results. If the edge is holding up and you're not seeing obvious "chippiness" then clearly it's in an acceptable range for that tool as used by you.

Re: Pictures of Various Honing Options

#32

Epic Pfeil

Patrick Chase

A few remarks:

I really like the Pfeil carving tools. I think that the hexagonal handles are very nicely proportioned, the steel is good, and they come very nicely finished out of the box. I'm even willing to pay WC's (admittedly exorbitant) markup. I have ~20 of them at last count.

"Chrome Vanadium" is an almost meaningless label. Some people take it as referring to AISI 6xxx series steels, but none of those are tool steels, so that's clearly not the case here (and there's a lot of variation even within that family). I think that the only thing you can conclude is that the steel probably contains more of Cr and V than any other element besides C and Mn [*]. That would rule out O1 (which contains more W than V) but it still leaves a huge range of tool steels.

Rules of thumb about hardness are very much steel-dependent. O1 gets very "crispy" as you go beyond Rc60. In contrast some of the modern PM steels hold good toughness into the mid Rc60s. PM helps because finer microstructures are tougher. Unfortunately we have no idea what Pfeil is actually using (unless somebody wants to spring for an analysis).

[*] Mn is almost universally present due to its role in "neutralizing" Sulfur contamination, so it's typically left unstated. For example several "Cr-Mo" steels contain more Mn than Cr, and all of them that I know of contain more Mn than Mo.

Re: Pictures of Various Honing Options

#33

Re: Hardness and cryo treatment

Warren in Lancaster, PA

I have a few Henry Taylor tools which were tempered lightly , at 375 Fahrenheit, so I suppose they would be around 61 hardness. I have used them in production work, white, oak, hickory, walnut and such and they don't chip. I don't really like them as much as tools that are more highly tempered. Some have suggested on these pages that a chisel used for chopping must inevitably either chip or fold, but I think a skilled worker has a pretty wide window where neither one occurs.

Reading some of these comments is like having someone trying to convince us that we really ought to like Bacos and powdered mashed potatoes or freeze dried strawberries better than the real stuff.

Re: Pictures of Various Honing Options

#34

Re: Hardness and cryo treatment

david weaver

Just guessing, I don't really know for sure how hard my iron is and how hard the AI chisels are, but I'd suspect the AI are around their hardness rating because of their behavior on a washita. 3 or 4 points of hardness makes a gigantic difference in feel on a washita.

As to the other things:

1) yeah, one never knows what chrome vanadium means. It's like the term silver steel in razors. At one point, silver steel (probably drill rod) was a specific thing....more than a century ago. Excellent for razors and would make wonderful tools, but none of the current makers really have the skill to work with it. Whatever the flavor of rod is that pfeil starts with, the results are excellent and I'd eyeball someone else's analysis, but I'd never fund it. Use tells me what I want to know. Presumably, their tools are just made in a die forging setup like a razor is made.

2) I don't know what the ultimate difference between Knight's irons and hock's are, but knight's are much better on beach's page, and in my experience, the same is true. The knight irons are at least as hard as the hock, so if it's not the cryogenic treatment (which I understand just accelerates the settling in plainer steels), there may be another factor. Knights irons felt icy on stones, hocks just hard.

My personal iron (made with starrett O1) is not very far short of hock hardness (I'll have to double check the last remaining hock iron that I have - if it's HCS, I can compare them on the washita today and tell instantly if they're within a point or so of each other). I thought maybe I had hardened mine around stanley hardness, but mine is harder. Because of a snafu, I didn't temper it, or I'd have shot for 350-375.

George's experience with O1 is that if you err on the side of high 50s rather than low 60s, you're more likely to get an iron that wears well. Maybe hock's iron would be better at 60, I don't know.

I got a chuckle last night when you talked about the carbide releasing monsters on Beach's page. You're pretty much making my point about there being no real benefit to those irons. I wouldn't have to ask warren twice or brian holcombe twice. If you keep at this and go more toward hand work, you're going to end up in the same place we have. It just happens. Brian's discussion . You get annoyed with the "benefits" of the other stuff, and find how reliable the genuine article is.

There's a wildcard with my iron, but I doubt it makes a difference. I couldn't get it quite as hot as I wanted, because my heat source is way too large, and it was burning me up heating the iron. I quenched it and never tempered it. I have no idea how it turned out as well as it did, but luck has something to do with it. Everything that I have tempered with O1 in the oven has been at 350 or 375, and for an hour, even though it doesn't need to temper that long. I have used my oven enough with a thermometer in various areas to know which places are actually the indicated temperature (the variation from front to back and in different spots is extreme, even on convection mode).

Aside from arranging a heat source, it's relatively easy to make irons that wear better than the Hock. It's not the kind of thing I'd skimp on O1 branding, because I suspect the difference is the quality of the stock.

(I have tried O1 straight off of the quench before, and it's as hard or harder than the hardest japanese chisels I've gotten - It can't be abraded appreciably on the washita).

Re: Pictures of Various Honing Options

#35

Re: Found one...

Howard Pollack

David- Do you have a way to get a description in English of the items on Buyee? When I press the translation tab only part, not a description of the item gets translated. Thanks.

-Howard

Re: Pictures of Various Honing Options

#36

Untempered O-1

Patrick Chase

O1 is about Rc65 as-quenched, depending on the austenitization temperature (it peaks at ~1500F) and assuming complete austenite-to-martensite conversion. As you say, right up there with Japanese tools.

Re: Pictures of Various Honing Options

#37

Re: Found one...

david weaver

Hi Howard - if you're using google chrome, you can just right click on a spot on the page and click "translate to english".

It'll do a better job than the site translator.

The only thing that won't get translated (obviously) is text that's on pictures.

Internet explorer has a similar function.

Re: Pictures of Various Honing Options

#38

Re: Hardness and cryo treatment

Patrick Chase

Edge life is a tradeoff between hardness-limited failure modes (folding), toughness-limited failures modes (chipping), and more complex modes like abrasion. When we speak of "optimal hardness" it depends on both the specific use and the user, and specifically which failure modes they tend to trigger, as I said in another post.

George and I have discussed this before on the other forum, and his argument is basically that in his experience, for his uses, and with the specific quality of O-1 he used, the best balance was just under Rc60. My experience is consistent with his for chisels, though as I said earlier I think that planes can go a touch higher because they aren't used for chopping and because the edge angle is typically greater, both of which reduce chipping and shift the optimum towards higher hardness.

What I'm trying to drive at here is that there's no inherent contradiction between any of our statements, because there's no single right answer. The optimum moves around as a function of all of the factors referenced above and more.

Brent's test that you referenced in the other thread emphasized abrasion-resistance, which is generally improved by higher hardness (though not as directly or exclusively as folding). I fully expect that use case to have an optimum that's a couple points higher than you might derive by looking across a wider range of WWing applications.

Abrasion resistance is an interesting and complex attribute because there's more than one way to provide it. That's what I was driving at when I said that abrasion resistance isn't as "exclusively" driven by hardness as is folding. If you buy into Brent's results you can see this by comparing Blue and, say, 3V. Tsunesaburo Blue is quite a bit harder, but Steve Elliott's 3V iron hangs in there very well indeed.

Re: Pictures of Various Honing Options

#39

Evolution of opinion

Patrick Chase

I think you may be misunderstanding where I'm coming from with the "carbide-ridden scratch-fest" comment (or whatever it was).

I think I'm pretty up-front that I take a very engineering-oriented approach to just about everything. You don't need experience to know with certainty that D2 and non-PM HSS and stainless steels are going to be marginal for anything that requires edge refinement. It follows from even rudimentary consideration of their properties, and I've therefore never had a particularly positive view of those alloys for most WWing tool applications.

Experience is a terrific thing, and never to be ignored because it almost always leads to deeper understanding in one way or another. With that said, the "voice of experience" also can't be accepted blindly or without due analysis and consideration. In particular you have to always ask what specific circumstances drove that experience, and whether they have been or can be changed in a way that opens new opportunities. When we fail to do that we invariably end up stagnating.

I think the different in our positions is that I don't subscribe to any particular dogma about steel "types" or sharpening systems. The same sort of analysis that tells us that D2/HSS/SS are problematic also tells me that some other alloy steels (particularly newer PM ones) can do very well indeed for WWing, and I'm not going to blind myself to that based on some quasi-religion about what is "right" or "traditional" or "natural".

Reiterating something I've said several times, my own "production setup" is actually pretty conservative: Mostly HCS, O1 and CTS-XHP [*] irons, and two-waterstones-plus-strop sharpening. I fully acknowledge that our community is far too quick to adopt "revolutionary, new, improved" geegaws that are of marginal value, but I also think there may be some wheat in that chaff.

[*] I label this "conservative" because while its manufacturing process is state-of-the-art, the alloy itself was expressly designed to be compatible with traditional workflows for sharpening etc.

Re: Pictures of Various Honing Options

#40

Re: Hardness and cryo treatment

David weaver

Patrick, you're telling me things that I worked through around 2009. I left that behind quickly when I started doing more making and sped up my sharpening.

George's chisels are harder. It's plane irons he's talking about tempering further.

Re: Pictures of Various Honing Options

#41

Thank you.

Howard Pollack

Thank you David. That is a very interesting site!

-Howard

Re: Pictures of Various Honing Options

#42

Re: Thank you.

david weaver

Howard - it's full of potentially gainful stuff.

In the mail yesterday (i flip stones, but I don't make any money at it so far, at least not in total), I got a $110 suita that is the strongest cutting suita I've ever used. I was hoping to flip it for $200. Now I've got to "grip it" instead. I have some more valuable stones that I guess I will be selling.

Anyway, here's the tip:

you can switch back and forth between translate, and find out what some Kanji are if you are looking for something specific.

For example, it wasn't very hard for me to figure out the kanji to "western razor", and then I copied the kanji in japanese and put it in a word document file. It's a lot more successful to search on the kanji than it is anything in English. You can just keep one file with all of the kanji you want to use in it with english translation next to it.

Re: Pictures of Various Honing Options

#43

420HC

david weaver

Sams had an offer a couple of months ago for a buck general and a buck 110 for $55. This is sort of strange, because the general price is $70 on amazon (or was), so I figured for the pair, I'd sell the general and cover both. There's some risk that doesn't work, but I sold my "general" for $64 on ebay and even after fees, I'm left with the 110 in 420HC.

The knife is not hard, but that's not a big deal. It's a hunting knife, you want sharp and you'll run into something with it sooner or later that makes you happy that it's easy to sharpen.

This is a picture of the edge on a dry washita (with lubrication, it could be finer). No large carbides in this stuff that I can see - it reminds me of 12c27 stainless. The "new" sharpening cycle here was about two minutes on the washita and two minutes on linen and then leather to remove the wire edge. Though the edge looks unimpressive, it shaves hair easily on both sides (because the edge is not quiet, but it's clean otherwise).

And though I no longer hunt, it would've been a fantastic hunting knife. Sharpens easily and would indefinitely on one stone and it's really functionally sharp almost to an extreme.

I have a chisel worked with iron oxide and one with a coarser honing paste, but my halogen bulb just quit, so maybe no more pictures today using the scope.

https://s13.postimg.org/thqlg601j/USB2_3_M_UE301000054_20171217144832.jpg

The two hunting knives that I've tried now that I really favor are the original camillus air force knife and this 110.

Re: Pictures of Various Honing Options

#44

iron oxide and cheap wax bar

david weaver

First, a picture of the .09 micron on balsa edge. This could be neater, but it's so slow.

https://s13.postimg.org/662hraj9j/5_micron_wax.jpg

Anything stray is left over from the LV green bar, which is what preceded this.

And something more practical - the 5 micron al-ox bar that comes from Mcmaster carr. I use this bar to buff things because it's got a little bit of tooth but still leaves a bright polish. The bar is a bit hard for applying (compared to the LV bar, which applies really easily with a drop of oil).

Hard to even figure out what to focus on with the microscope while taking pictures. the edge is rounded a little bit from the softer surface, I guess, and it just sort of disappears.

Of tehse two, I'd choose the yellow bar from mcmaster carr - it's super fast and pretty good. A stray scratch here or there, but not sure they'd ever show up on a surface.

https://s13.postimg.org/nw46cbp4n/ironox.jpg

(pictures are at 150x).

Re: Pictures of Various Honing Options

#45

Re: iron oxide and cheap wax bar

Patrick Chase

The McMaster bar is made of friable calcined/tempered alumina, similar to the alumina in the infamous green Formax bar.

It will therefore tend to break down and become finer-cutting in use (again like the Formax bar) so the results depend a lot on how you use it. I think that's why McMaster bills it as a combined cutting/polishing compound rather than just one or the other. I don't have direct experience with it but expect that in practiced hands it could do a very creditable job.

5 um is about 2500 grit, which is already good enough for many purposes. Work it in a bit to break things down and you're probably up to 5K or so.

Re: Pictures of Various Honing Options

#46

Re: iron oxide and cheap wax bar

david weaver

That's definitely a flaw in my screwing around here. I'm using a fresh section of wood and applying the stuff to avoid contamination, but that means the abrasive is all out to start. It's actually kind of nice. If you open the kitayama picture and compare it to the gold stuff from mcmaster, the gold stuff fares quite well, but it's less uniform.

My own personal strop with stuff on it (which has always been dursol until scraping it off and replacing it with autosol), I've always noticed how much more docile it is once the "stuff" is settled in. Of course, a strop like that glazes over, as does my prized chrome ox strop for razors (that I keep out of the shop). A drop of oil on either one will wake them up a little, but you start all over each time you load a strop.

All in all, it doesn't really matter. what I don't know is whether or not the rounding that inevitably occurs at the very edge with chrome ox or iron ox due to repetition negates the refinement over a faster compound. It'll never matter, of course.

If I can manage to keep track of myself with my iron and others planing, I will try to get pictures of edge wear between them and A2 to see what the wear looks like.

Re: Pictures of Various Honing Options

#47

Re: 420HC

david weaver

This is a knife that would benefit from honing compound or a finer synthetic stone, but it's hardness is established for easy sharpening and cutting meat. On anything else, I don't think it would hold that refinement for long.

I see what looks like little carbide voids on the blade (and it's possible that the washita is becoming a notorious carbide grip it and rip it (out) stone), but they're little.

I'm tempted to go back and work through the fallkniven knife on a diamond hone and then on the (diamond loaded) brass bar to see if I can burn through the bubbles on the surface. Shapening a knife on that combination is like gnashing teeth, though. Metal on metal.

Re: Pictures of Various Honing Options

#48

Re: Evolution of opinion

david weaver

I sat on this yesterday, because I have a (sounds different than I intend it) statement that I used to make on another forum that always got peoples' hackles up. "Hand Tool Woodworking doesn't need more Engineers" or other variations on that.

I'm not intending to slight engineering, as essentially all product development that makes life easier is some variant of design or engineering.

What comes to mind is that 99% of what makes us bad woodworkers, and most of us are - me included - has nothing to do with lack of engineering. It has to do with our intellectual laziness in forcing ourselves to understand design, take risks on things that aren't black and white and be educated about them.

Hasluck's book on carving comes to mind (because I haven't read many books, I could only pick about 6 legitimate woodworking books that I've read in earnest), the discussion on the engineering side of things is pretty slim. the discussion of proportion of carvings, what makes them life like, etc, isn't. The trouble is when we're sitting at our desks at lunch and we want to "solve a problem", it's easier to ponder things like no more sharpening, or buying something else to try. I'm just as guilty.

What I should have is a tablet and force myself to learn one new thing about design, one new competent move with the skew, etc, per day.

i can't say I don't use anything that was engineered relatively recently - I love the CBN wheel. I love the FEIN turbo III, but I don't wish for a lot of the kinds of things that used to come up in discussions on here nearly a decade ago. For example, Bill T. was really looking hard at trying to make something you hardly had to sharpen. It went so far as questioning whether or not irons could be made with a smooth titanium nitride coating on the back so that you would only ever have to sharpen the bevel.

The exasperation isn't so much about engineering in general, it's just the merry go round that comes around over and over. And there was a fair period where I did it, too.

Re: Pictures of Various Honing Options

#49

Re: Evolution of opinion

Patrick Chase

I actually don't completely disagree. As I've said a number of times, I Keep It (Relatively) Simple (tm) when I'm actually trying to get stuff done as opposed to yakking on forums or conducting silly experiments.

With that said, if you really had the courage of your convictions then I'm not sure you'd be pointing a metallurgical scope at your edges :-).

Re: Pictures of Various Honing Options

#50

Re: You're right..

david weaver

..The scope has been a tremendous waste of time, but it has satisfied my curiosity a bit.

I got it to look at razors, though (for that, it's excellent, because they're a lot harder to get right quickly when they've never been sharpened before or when they need a lot of geometric work). The 16 degree bevel makes them delicate and much more quality sensitive, so the scope is nice to have to both see the edge when sharpening, and to inspect it for defects.

But a waste of time on the tools! And I'll go back to using the washita or a fast suita (which make the coarsest looking edges of the pictures I've taken).