its hot with bubbles

Posts

its hot with bubbles

#1

its hot with bubbles

Darrin Hill

75 % humidity average 100 degrees...

this is what happened when i got sidetracked after spraying on some deft high gloss...


img

Re: its hot with bubbles

#2

Rob Wallace

Re: its hot with bubbles

Rob Wallace

Hi Darrin!

I have had this happen when spraying lacquer (interestingly, also Deft gloss lacquer, but I don't think the phenomenon is brand-related).

In my case, when this has happened (more than once), it is related to the high temperature AND having the piece exposed to direct sun while drying. Spraying pieces (outdoors) in the shade works fine, without any problems, right next to pieces exposed to the sun which "bubbled" (i.e. pieces are at the same temperature; only difference is direct sun). Extra heating of the wood/lacquer by the direct sunlight likely expands air trapped in the wood probably builds enough pressure to form the bubbles (for me, they only happen "on the sunny side").

To repair this, I simply waited a few hours until the lacquer bubbles/surface had hardened, then sanded-off the bubbles with 240 or 320 grit abrasive to level the area. A quick dab (to create a thin film) of lacquer thinner flattens out any irregularities left by the "bubble rims" or the abrasive; allow to dry completely if you used the thinner. You can then re-coat with several thin layers of lacquer (which "melt-in" to the lower repaired layers), and you're back in business.

Been there - done that. Stay out of the sun!

Rob

Re: its hot with bubbles

#3

Re: its hot with bubbles *LINK*

mjonesrdg

Darrin,

The link will take you to Wood Finishing Supply's page on troubleshooting lacquers. I will add, that, shooting a brushing lacquer works just fine IF you give the shot surface a lot more time between coats. The brushing lacquers (such as Deft Gloss) contain a retarder, and if you put a coat on top of a coat that has developed a film (not tacky) but has not completely cured out, blisters will appear. Your high temps and high humidity may have exacerbated the problem, but the primary culprit is the retarders in brushing lacquers.


http://http://www.woodfinishsupply.com/LacTroubleShoot.html

Re: its hot with bubbles

#4

Deft

Mark Mandell - Gone Round In New Jersey

markets a lot of rattle-can spray lacquer as well as non-retarded quarts. It's not just "brushing" lacquer.

The problem appears to be too heavy a spray coat with not enough time to allow evaporation of the main carrier solvents. At a 100°, it doesn't take much to "boil" a high-solvent, low-solids lacquer like Deft.