Does anyone have an easy heat treating process they are willing to share? I have some O1 drill rod that I would like to make into gouges. The machining is not a problem but not sure about the heat treating.
When Alan Laser came to our club he showed us how to treat a hook tool he uses but it was several years ago and I don't remember the process.
It's very simple. Heat it red hot until a magnet won't stick to it. This is the critical temperature. Ideally you need to hold it at that temperature for awhile but I've had very good luck quenching it after holding it there for just 10 or 15 seconds.
Since it's 0-1 it needs to be quenched in oil. Used motor oil is fine but I use Peanut oil. It has a higher flash point so it's less likely to catch fire and it's very safe to dispose of. Either way you need to do this outside or at least well away from anything flammable. Dump the red hot area completely under the oil. This reduces the chance for a fire. You will still get a lot of nasty smoke which is another good reason for doing it outside.
Now it's too hard and needs to be tempered. You can do the blacksmith thing of heating it until it's straw colored. polish the metal first so you can see the straw color. This is challenging if your not used to it because the thin areas will heat faster and you can easily turn them blue which tempers it back too far and it won't hold an edge.
It's much easier to just put it in the kitchen oven at 425 degrees for 1/2 hour per 1/4" of thickness. Then just turn the oven off and let it cool naturally. It should be a light straw color which is good enough for our purposes.
One question. One half hour per quarter inch of thickness means where. Are you measuring the total thickness of the rod or the thickness at the bottom of the gouge?
Skip I'm not sure. I remember reading that when I studied heat treating drill rod. You can't hurt it by going too long so I would err on the side of maximum diameter. The temperature actually varies from about 350 to 450 depending on how hard you actually want the cutting edge. To know for sure you need to order the heat treating directions for the rod you buy. You can get it from the dealer. I picked 425 because that's a rough estimate for the hardness needed for most turning tools.
The time isn't critical, temperature is. If you use a kitchen oven, temperature can fluctuate quite a bit so it is a good idea to verify the temp with an oven thermometer and add some thermal mass to even the temperature out (I use an old cast iron dutch oven filled with sand). It won't hurt to do two cycles of an hour each. It doesn't have to cool naturally, you can dunk the piece in water to cool it between cycles.