Re: How To Drill HSS?
RussFairfield
>Why don't you make life easier for yourself and make the hollowing tools out of a carbon steel? It can be about the same hardness as an M-2 HSS with a lot less effort.
Drilling HSS can be done a lot of ways in theory and according to the advertisements. Some HSS can be drilled with a carbide masonry bit running at a slow speed and using a lot of oil as a coolant. Your "hot nail" method can be used to destroy the hardness in a local spot, but you will also risk altering the metalurgy in the rest of the bit. The "hot drill" has the same problem.
My experience with all of these methods is that we will reduce the HSS to no better than a hardened carbon steel, and sometimes not as good; and we will have wasted a lot of effort doing that.
A better solution is to use a hot saw to make a slot from the enge to the center of the bit.
To use a carbon tool steel, do the drawing and hardening steps, but omit the tempering.
It can be annealed by heating to Cherry Red and allowed to cool in still air. That makes them easy to drill and grind to any shape you want.
Then heat them to the same Cherry Red and quench in oil or water to reach maximum hardness. Omit the drawing back. The steel will be brittle, but that is OK for a hollowing tool bit that is supported in a holder.