Re: My Method
Mark Mandell - Gone Round In New Jersey
I've laid up a bunch of mica and never had a failure. The first thinned coat penetrates into the wood surface better so the bond with the wood is more than surface stickum, and does a better job of wetting out the laminate surface as well. Multiple coats is the key here as you wind up with the same amount of glue coating, but with the glue layer even. This is really important when working with thinner laminates.
My reference to a "sheen" may have been a bit misleading. I'm not talking about what you'd see with a coat of thin shellac sanding sealer. On plywood it will take at least 3 applications to get a real shine such that any wood texture is hidden under the glue. Same for the laminate. Think "finished" table top with the dried coating several mils thick on each part.
Couple of points:
a. Since we are in the humid Summer, care must be taken to allow a coat to dry before recoating. Otherwise you risk blushing (just like with lacquer) which will trap condensed moisture between the glue layers and weaken the bond.
b. Putting extra around the edges is fine, but again, you want just enough glue to make a strong bond. Too thick a layer at the edges can lead to degrading the glue over time and you'll get the laminate lifting, especially at the corners.
c. I prefer the "team" approach (4 hands) to putting the laminate down on anything over 3' in any direction. I bend the plastic into a "C" shape then position it along one edge with an even amount of overlap, then press it down onto the surface letting the C straighten out as you roll it on along a line away from the first contact edge. This prevents trapping any air under the laminate which, once the sheet is down, will not roll out. Any air bubbles will be there forever DAMHIKT 
I worked in a factory shop one summer and they used spray applicators as well (hand application takes too long on a production line). They also adjusted the glue viscosity depending on the weight of the laminate being used and a roller press to put laminate to prepared substrate with a lot of pressure.