When using it for glue, I use wood flour, the super fine stuff that cakes the inside of an upper DC bag (or filter cartridge). Add what you need to get the consistency required. Epoxy is thixotropic (sp) in that with the right amount of bulking agent added, it won't run or sag, and will work like paste. There are, of course, specific fillers you can buy like micro-balloons etc., that won't color the resin, or you can ise different color wood dust to help blend color. Procedure is to mix your resin and hardener, then add the bulking agent.
Bill, There are many options, but the one I use most, is Colloidal Silica. It is a very light weight powder, which does a good job of thickening without adding weight, which is nice when using such a slow setting liquid, subject to the laws of gravity. A 5 oz container, is about the same volume as a 2 # coffee can.
It changes the the clear or amber color to a light beige, when I add about half the cubic volume into a given volume of liquid. Keep adding, and it may look like cake icing, which turns into a hard plastic when set.
Around the shop for furniture, I also add to that wood dust from my belt-sander bag to match the color of the surrounding wood. You could use just the wood dust, but it ends up a lot darker than I usually want, plus it is heavier and more brittle, which is another benefit of the colloidal silica, makes it less brittle.
Fairing compound makes it easier to sand, for getting rid of lumps and bumps under a painted surface.
Graphite powder makes a good slick surface.
The best advice I can give to any new user of epoxy, is to ask for a user manual with you first order, and read all of it, even if you only need a little of the information. Knowing the other stuff will open new possibilities, and add to your bag of tricks.
In the thread below, one poster stated that epoxy doesn't stick well to itself, which isn't the case, unless it was over a highly polished surface. But dulling any hard surface with a sander, giving the epoxy tooth, will make an excellent bond.
There are several traditional products used for thickining resins/epoxies and each has a particular advantage.
For tooling or in situations whare you will be sanding or shaping the curred resin, talc is used as a thickener. Talc is soft and as you might expect it makes the cured resin easier to sand than if you had not thickend it or thickened it with something harder.
Wood flour can be used as a thickener and it performs similar to talc. Some people don't care for wood flour if the finished product will be used around water, I have never had a bad experiance when using wood flour.
By far the two most popular thickeners in wide use are micro spheres and cabosil. Micro spheres are tini hollow spheres of glass and cabosil is fumed silica. Micro spheres may be slightly more popular only because it is slightly easier to work with. It is a very fine powder, and while being light weight it lacks the extreme airbore tendancy that cabosil has. Cabosil has a slight strength advantage over micro spheres but it is such a fine particulate that it becomes airborne just opening the container. And since cabosil is a silica you need to take safty precautions not to inhale the particles or you risk contracting silicosis.
All the products Iv'e listed should be available from the same supplier where west system is sold. if they don't carry them look to a boat building supply house or other fiberglass supplier.
In a pinch I have even used plaster which worked just fine.
My experiance with coloidal silica was when doing ceramic shell bronze casting. the colodial silica was a liquid. and we added silica flour to it to make the slury, but the last dip was into pure colodial as a binder.
Not sure if there are other types of colodial silica.
I want to stress the air borne nature of the silica and to perhaps a lesser extent the very fine wood flour. Be very carefully and wear an excellent mask and remember that it might float in the air much longer than you think. The extremely fine stuff it the worst type and it is the most likely to get into your lungs. I think the state of California thinks EVRYTHING is a Carcinogen but in this case perhaps we should listen.
As far as I know neither silica nor wood flour are carcinogens. Silica and specifically cabosil still poses a SIGNIFICANT hazard to your health. Silica is dangerous in the same way that asbestos fibers are dangerous. With silica the tiny particles resemble little pieces of glass and when these enter the lungs they are drawn in a tiny bit further with each breath. This causes the silica to tear tiny canals in your lungs which heal and form scar tissue. Eventually when enough healthy tissue has been replaced with scar tissue your body will not be able to get enough oxygen. There is no treatment for this and the silica cannot be removed. This is called silicosis it is serious and for anyone working around sand or even some types of clay it is a very real risk that can be eliminated by wearing a good respirator.
Either way, I don't want it, and don't want Bill or anyone else here or in the wide world to get it from something that seems as innocent and harmless as wood dust or sand or whatever.
I myself don't need no stinking respirator because I hold my breath the whole time I am working in the shop. That's not true. I actually only exhale if I can't hold it long enough.
I don't know if "wood flour" is the same thing as "wood dust," but wood dust is a recognized carcinogen. Do a quick search on Google and you'll find a number of hits relating to wood dust as a carcinogen. Here's a link to the Health and Human Services Dept.'s toxicology study of wood dust that sums up the then current research on the matter (the report was submitted in December 2000).
Sorry about the post. I'll try again. It comes up as a PDF file. If I fail again, GOOGLE "National Institute of Health wood dust final report." It should be the first link that comes up. Here's the link (I think):