Gold leaf sealer?

Posts

Gold leaf sealer?

#1

Gold leaf sealer?

Norm Smith

Hi all,

I cannot find the sealer paint or whatever that goes under gold leaf. What paint can I use?

Thanks,

Norm

Re: Gold leaf sealer?

#2

Re: Gold leaf sealer?

Keith T

Hi Norm. Gesso, I apply several coats, sanded between coats. Red oxide primer adds some pop over the black gesso. Size (glue) is available at art stores, don't use craft store variety...NG

Re: Gold leaf sealer?

#3

Re: Gold leaf sealer?

Norm Smith

Hi Keith,

Thank you so much. That is exactly the advice that I was looking for.

Norm

Re: Gold leaf sealer?

#4

Re: Gold leaf sealer?

Chuck Engstrom

Hi Norm -- For oil-based gilding you can use spar varnish such as McCloskey's Man o' War, MinWax Spar varnish, or other oil-base varnish. Real gilder's varnish is available from the gilding supply outfits such as Sepp Leaf (check their "Workshop page" at http://seppleaf.com/sgw) and others but oil-based spar varnishes will do just fine. Be sure your base surface is well sanded and sealed with a couple coats of shellac before applying varnish.

In either case you wait till the varnish is almost dry before applying the leaf. The test of readiness is to very lightly graze the back of a finger across the varnished surface -- when your skin sort of jitters across the surface, it's ready. If your finger still sticks as though passing over drying honey or maple syrup, it's still too wet. And if your skin doesn't drag at all, it's too dry and you can just try again with a fresh coat.

Real gilders varnish comes in 3-hour and 12-hour formulations, which means that it would be "ready" (as I describe above) 3 or 12 hours after you brush it on. There is some variation on this, of course, depending on ambient conditions of temperature and humidity. I thought I had better luck with the 12-hour variety, which seemed to stay "right" for a longer period if I was working on a larger project. The spar varnish will probably be ready in a couple of hours.

There are acrylic varnishes at Michael's and A C Moore but they go off much faster, as I recall. I tried some one time but can't remember much more about it than that.

Water gilding is another whole process involving more ancient methods with a greater learning curve than oil process. I haven't done any gilding at all lately but I just now finshed watching Jimmy Clewes' DVD of the oriental box with gilded interior and so may be doing some again soon. Because you have to work carefully and deliberately, it imposes its own variety of relaxation, I find.

I do have a DOC file describing the procedure I learned and will be glad to pass it on if you wish.

Good luck with it. I'll look forward to seeing your results.

Chuck Engstrom

Re: Gold leaf sealer?

#5

Re: Gold leaf sealer?

Norm Smith

Chuck, I would sure appreciate the file. Would you send it to the following address nrsmith@syd.eastlink.ca

I will let you know how I get along.

Thanks,

Norm

Re: Gold leaf sealer?

#6

Re: Gold leaf sealer?

Mac Ray

Hi Norm, I have found that the 12 hr. size generally gives a better hold out or gloss to the leaf...I always run a test panel to check how long the size takes to dry before I go ahead with the final gilding......I also prefer fresh Spar varnish as a size...if things don't go well on the first try,let the size dry THOROUGHLY, and then start the process over again,sometimes it can take up to three tries to get what you want .....all worth the trouble...nothing looks like the real thing...........