#1

Dick Hines

One more for Mike

Dick Hines

>Another madrone box. This is the last piece I am out of madrone, for now. The box is 2 3/4"D X 4 1/2"H.

The finial is #6 ground wire, . What else. I ground it to a point and then heated it to cherry red. The bent it. Once it is worked it will reharden.


img

Re: One more for Mike

#2

Mike Stafford

Another hot BOX!!!

Mike Stafford

>Dick, you may the first to incorporate wire exactly this way into your turnings and they sure do make a statement. I am surprised at how versatile a material wire is. Next you need to figure out a way to patinate the copper wire so it develops that wonderful verdigris color. I think that might look great on the right woods.

A terrific box, Dick. You are giving me ideas....I might have to use some big aluminum wire I have...Just kidding!

Re: One more for Mike

#3

Dick Hines

Re: Another hot BOX!!!

Dick Hines

>I hear copper will turn green if you pee on it.

Re: One more for Mike

#4

Re: One more for Mike

Cyril Griesbach

>Wow, Dick, that's just great work...both of them. Please find another way to patinate that wire.

Re: One more for Mike

#5

Mike Stafford

I ain't buying that box.....!

Mike Stafford

>I'll let you do the experimenting but I am sure I don't want any boxes that are the result of those tests.

Re: One more for Mike

#6

Dick Hines

Re: I ain't buying that box.....!

Dick Hines

>I have forun a place that sells chemicals to put patinate on copper. Ordered some this evening.

Re: One more for Mike

#7

Re: One more for Mike

charlie belden

>From my jewelry making days

Oppi Untract's Bool - Metal Techniques of Craftsmen copyright 1968

Rich Reddish Brown on Copper

Copper sulphate 120 grains

Water 1/2 pint

Dissolve copper sulfate in water, heating if necessary to dissolve the copper sulfate.

Neutralize the solution with sodium nitrate

then add 150 grains of red iron oxide. Immerse the article in the solution until its color starts to change. Remove and heat on hot plate to deepen the color, Repeat for even deeper color.

Antique Green on Copper

Copper nitrate 4 ounces

calcium carbonate 4 ounces

Ammonium chloride 4 ounces

Water 1 gallon

Warm the article as well as the solution. Stipple solution on object with cloth or sponge. For color variations, immerse the treated piece in clean boiling water AFTER the green has developed.

Yellow-Green on Copper

Copper sulphate 48 grains

Ammonium chloride 48 grains

Calcium chloride 48 grains

Water 3 ounces

Applied with a brush and allowed to dry - 3 applications produces a uniform green patina

Bronzing Copper

Copper sulphate 400 grains

Water 2 ounces

Use warm, immersing object two or three times, wire scratch brushing between immersions. Depending on the purity of the copper the color may be light brown, terra cotta, purplish or dark brown.

Most lapidary and jewelry supplies shops carry "liver of sulfur" - yellowish rotten egg smelling lumps. Dissolved in hot water, produces browns to almost black on copper and bronze as well as sterling silver (which has copper in it).

Now I just have to remember if the "grains" are a unit of weight for weighing pearls or a unit of weight in the troy system (28.8 grams/troy ounce, 20 penny weights (dwt) per troy ounce, 28 grains per penny weight.

You get to do the math.

Re: One more for Mike

#8

Steven Antonucci

Vinegar and salt will do what you want

steve antonucci

>

Re: One more for Mike

#9

Mike Stafford

A much better solution than Dick's idea, Charlie!

Mike Stafford

>

Re: One more for Mike

#10

Dick Hines

Re: A much better solution than Dick's idea, Charl

Dick Hines

>But Mike it is not as much fun, like writing your name in the snow.

Chemicals are on order.