buffing a shellac finish

Tom Sontag - St. Louis

>While my project is not round, I come to y'all for buffing expertise. I padded on some shellac, one or two fairly light coats, and proceeded to buff them out with the Beall system on my lathe. I am going over some highly polished (12,000 grit) woods like osage, persimmon and African blackwood. I really like the way they look this way.

When done and held at the right angle, I notice linear streaks probably from the tripoli stage. The shellac has lost its padded marks but taken on some furrows from the smoothing stage. I could actually live with the result, but maybe things could be even better.

-How long do you let shellac cure before buffing?

-Am I pressing too hard when buffing? I doubt it; I barely deflect the buffing wheel fibers.

-If long, is there an intermediate step before the tripoli wheel to smooth things out? Going at it with very fine sandpaper seems a sure way to clog the paper in a hurry.

-Maybe my shellac should be even more diluted so there is less finish to buff?

Re: buffing a shellac finish

#2

Re: buffing a shellac finish

MFoster

>I used shellac to finish a segmented piece to a high lustre. Nice thing about shellac is that it fills the pores well and is easy to build a nice film that can recieive a high polish. I found that buffing did the same for me as what you experienced. This was at least a month after the final layer of shellac. It could be that there was still some alcohol trapped in the finish which left the film slightly pliable. It was my thought that buffing was generating heat that caused the streaking. I resorted to using only hand polishing, as in French Polishing. Be interested to find out if anyone knows if heat from buffing will melt the shellac

Re: buffing a shellac finish

#3

Re: buffing a shellac finish

John K Jordan

>Heat will soften shellac and make it flow. This is the basis for friction polish. When buffing friction-polished surfaces on rare occasions, I try to use a very light touch. But you said you are already doing this.

Another thing which can mess up the surface is too much buffing compound or too much wax.

If using shellac on a turning (and not as friction polish) I do tend to thin it quite a bit with alcohol and apply several coats.

I'm wondering if hand-polishing with pumice and rottenstone would work better for your situation, perhaps with a different finish over top the shellac such as oil or lacquer.

JKJ, certainly no expert

Re: buffing a shellac finish

#4

Consider skipping the Tripoli

David Walser

>Tom,

Have you considered skipping the Tripoli and starting with a less aggressive compound, such as white diamond? The Tripoli is supposed to scratch the surface of whatever you're buffing. It sounds like that's what it's doing. If you don't want it to do that, don't use it.

I'm just guessing. If I'm wrong, I'll double your money back.

Re: buffing a shellac finish

#5

Re: buffing a shellac finish

Russ Fairfield

>I am questioning why buffing is necessary. Properly done, a French Polish should have the highest gloss possible from shellac, or any other finish.

The problem with buffing is that Shellac is very sensitive to heat, and it is easilly damaged if it is still soft. It takes a long time for shellac to reach its full hardness. You should wait at least 2 weeks before buffing, and you will really notice a difference if you waited 6 months to a year.