Home Articles Forums Gallery Marketplace Videos

WoodCentral Forums

Knowledge You Can Build On — Est. 1998

Reach the woodworkers who ACTUALLY BUY

Kiln drying question

Posts

Kiln drying question

#1

Kiln drying question

Gary in Zirconia, NC

>I got to wondering. Why is it that we put sealer on our blanks to let them dry slowly so they won't crack and others put their blanks in a kiln to dry them fast and they don't crack? Do the kiln drying people put sealer on their blanks? Do they have more or less losses from cracking?

Re: Kiln drying question

#2

Re: Kiln drying question

Russ Babbitt

>Kiln drying is done under controlled conditions of temperture and humidity. Different conditions for different woods. Turning wood, such as bowl blanks, are usually too thick for kiln drying so we look for alternate methods. Also most of us cannot afford kilns. Unless you would like to gut a household freezer put some holes in the top and low watt bulb in the bottom and put you blanks and roughed out bowls inside. This method, like others, work for many of us.

Re: Kiln drying question

#3

Re: Kiln drying question

Bart Rhoads

>I have been using upright freezers as kilns for drying bowl blanks going on 7 yrs now. Like the other thread stated, all it amounts to is a upright freezer with a couple of holes at the top and a 2" hole at the bottom. I regulate the humidity by closing off 1 or 2 of the holes at the top and I have 2 60 watt light bulbs for heating. Any insulated box will work though. I turn my bowls or whatever I am turning with a wall thickness of about 10% of the dia. I just turn my blanks and load up the kiln, shut the door and forget about it. Most blanks will dry in about 3 to 4 weeks. Some wood, such as mesquite will dry in about 2 1/2 weeks. I would imaging this will vary depending where you live. Most of my blanks will come out flaw free, depending on the type of wood. But I figure on losing a few now and then. This has always worked for me. And I dont have to contend with sealing, bagging, boiling or soaping.

Re: Kiln drying question

#4

Re: Kiln drying question

Jim Swank

>It's not a matter of how fast they dry, but how nearly equal you can keep the moisture content throughout the wood during the drying process. Wood shrinks as it dries. If the outside dries faster, it shrinks faster and checks or splits.

The easy, low tech, and slow way to do this is to use some combination of sealers and barriers (bags) to slow down the drying process. The goal is to not let the outside dry any faster than the interior moisture can migrate to the outside.

The high tech way is to raise the temperature so the moisture will migrate faster, and control the humidity to control how quickly the outside dries.

The goal in either case is to maintain equilibrium moisture content (EMC) throughout the wood.

Re: Kiln drying question

#5

Brad Vietje

Great Response

Brad Vietje

>I'd also add that rough turning the bowl first is the key ingredient in either method. You'd have very little success drying a 5" thick bowl blank or half log by ANY means, but turning the form down to 10-15% of diameter and avoiding the pith will help avoid problems, and in many cases, is all you have to do. Extra precautions or steps are determined by your climate, the wood species in question, and how soon you need the finished product.

Safe spinning,

Brad Vietje

Newbury, VT

Re: Kiln drying question

#6

Thanks to all

Gary in Zirconia, NC

>