>I apologize for the photo. I only had 15 miunutes to shoot these guys today. I carve the rim on this one because I couldn't possibly keep the bark on. this is for a gift for our secretary who is getting married this weekend.
>John, that's a beautiful cherry bowl. It brings up some questions in my mind. Was it cured when turned... or was it green? The reason I ask is that Cherry cracks really bad in my hot, dry, shop, and with the pith from the tree in the centers of the bowl, it makes me wonder how you kept it so crack-free.
A long time in the soap and alcohol soak is the only way I can think of that would keep it from cracking. Just curious.
>I don't subscribe to all the different soaking methods. Not because they may or may not work (I think Dave has proven they do) it's just that I don't want all the mess and fuss of boiling, soaking etc. I did my best to save all the Cherry. Most of it checked beyond use. I don't have a good place to store wood. It sits out in the sun which is probably the worst thing you can do. To save this piece I cut it to shape larger than I wanted sealed it with endgrain sealer and then put it in a plastic bag. Sealing it with endgrain sealer only slows the damage down a tiny bit on cherry. I stored it this way for a month turning the bag inside out whenever I though about it.
I turned it in one setting down to 7mm thick. I put it in a plastic bag for a week turning the bag inside out every morning. Then I would open the bag and let the bowl sit for the evening making sure it was out of the sun. After a few days of this I just let it sit out. It dried completely in 2 more days. I'm not sure the plastic bag is necessary, possibly just putting in a box or cabinet to keep the air movement to a minimum would probably work but I'm always worried about fruitwoods so I take extra caution.
I put the piece back on the lathe with a vacuum chuck and power sanded with the lathe off.
>Allen ON woods that I think might be a problem I usually shoot for a wall thickness of 3/8" or less. If wood can move as it dries it is less likely to crack. My friend Randy and I made a bunch of goblet sort of shapes out of different woods like Apple, cherry, holly, pine, and other woods we had handy that were prone to cracking. We chose woods with knots and swirly grain. Anyway we turned one each to 3/8" and one to 1/8". The 1/8" pieces warped more but had little or no checks even in the knots. The 3/8" pieces had considerable more checking. I had read this but wanted to find out for myself.