Re: Tool steels - Part 1
RussFairfield
>It just happens that I have a rather long article in my working file. It follows in its entirity. There is a follow up and that is in the next message. My analogies will drive a metallurgist nuts, but that will be their problem.
Points to ponder - #1
Too many woodturners are looking for that magical tool that never needs sharpening. Like the 200mpg carburetor, they think that modern technology should be able to provide this to them. The tool manufacturers have capitalized on this desire with "new" tools that are sold on basis of advertising claims such as "new and better", "Powdered Metallurgy" because it is better, "durability", greater hardness, and a lot of technical terms that nobody understands. It must be working because all of the catalogs are filled with these tools. They are purchased solely on the basis that they don't have to sharpened as often.
We never consider such things as whether the steel alloy is even suitable for use as a tool, that it may be too brittle for a small diameter tool, how sharp and edge we can get on it, what grinding wheel and speed should be used, or whether we should be using a coolant for grinding these steels. Only Jerry Glaser and a few lesser known manufacturers have continued to make turning tools whose metallurgy is matched to the size and use of the tool.
Making a scraper from the new high-alloy steels is a step in the wrong direction. I doesn�t matter if the burr is put on a scraper with the heat from a grinding wheel or by displacement of the steel at the edge with a burnisher, the sharpness and quality of the burr decreases with the increasing alloy and particle sizes in the steel.
We can use a rather simplistic analogy. Think of a piece of high carbon tool steel as a package of "corn flakes", and the high alloy as the same box filled with BBs and golf balls. When softened by the heat from a grinding wheel, the "flakes" at the cutting edge are bent upwards to form a burr that is the thickness of a single flake that is still attached to the other flakes in the package. The "flakes" have enough ductility that they can also be bent with the pressure of a burnishing tool.
The farther we get away from the box filled with "flakes", and more towards the box that is filled with BBs and golf balls, the more difficult it is to form a thin burr on the edge. Some of these high alloys will have 50% of the flakes replaced by the BBs and golf balls, and there aren't enough of the "flakes" remaining to form the burr.
Using a burnisher depends on the ductility of the steel. The higher alloys have a stronger bond between the BBs and golf balls, they are less ductile, and it becomes more difficult to move the metal as their number increases.
We have to consider what we are trying to do. These tool alloys were developed for cutting steels and not wood. The machanics are different. When a steel is cut with a tool, a small crack is propogated ahead of the cutting edge. The tool wear is then the result of errosion of the tool surface behind the cutting edge. It is not unusual to have a burr of metal bonded to the cutting edge to fill the void that is created by that small crack.
Wood is separated by two mechanisms. The cellulose is either sliced with apart with a very sharp edge, or it is ripped apart with a tearing action. We can use the comparison of "shearing" a sheet of paper with a scissors as opposed to "tearing" it apart with force. We would always prefer the "slicing" to the "tearing". But the "slicing" starts to become the "tearing" as the edge loses its ability to cut through the fibers. It doesn't matter whether the change is because the edge of the sharp "flakes" has worn away, or that the edge was never sharp because it is filled with BBs and golf balls, the result is the same.
This same analogy can be applied to describe the differences in the cutting edge in a "sharp edged" tool that doesn't require a burr. It has to do with the sizes of the particles and how many of them are in the alloy. The edge of a single flat "flake" of steel is sharper than that same edge with a lot of BB's and a few golf balls in it. These BBs and golf balls are harder and will wear less than the "corn flakes", but they will never be as sharp.
The far end of the alloying spectrum is a "carbide" where all of the flakes have been displaced from the box and it is filled with nothing but the BBs and golf balls. They are bonded very tightly together, they are very durable, but they don't make a very sharp edge for "slicing" through wood fibers.
Where we want our tools to fit into this specturm of "corn flakes" to BBs and golf balls is the choice of the user. My choices are as follows....
SKEW -
This is a tool where the sharper the edge and the smaller the bevel angle, the better it cuts. It is impossible to make the edge of a skew "too sharp". For this reason, any alloy greater than an M-2 HSS is detrimental to having a "sharp" tool.
SCRAPERS -
High Carbon steel makes the better burr, but M-2 HSS is a good compromise between the sharp edge and durability. An M-4 steel is marginal, and anything of a higher alloy than that is a waste of money because the tool is no longer useful.
GOUGES -
An M-4 or similar HSS is the best compromise between durability and sharpness for most turning, and I have slowly replaced nearly all of my gouges with the M-4.
I have a 3/4" diameter high-alloy that I reserve for roughing cuts on large pieces, abrasive woods, bark edges, and nails; all places where I want a durable tool and the surface finish and tear-out aren't important. This is also a large diameter tool where strength is more impoprtant than flexibility, and I sometimes wish that I had one of them that was 1" diameter.
I still use a High Carbon tool steel as a finishing tool for spindle work because the sharper edge will leave a smoother finish on the surface of the wood.
PARTING TOOL -
Like the skew, the parting tool is better when it is sharper. I use a parting tool a lot for spindle turning, and the quality of the cut is important to me. For this reason, I prefer an M-2 steel for this tool. I purchased a 2030 alloy parting tool, but the sharpest edge that I can get on it is about where I would take the M-2 tool back to the grinder. There is no advantage in having an almost dull tool that will stay that way for a longer time.
ROUGHING GOUGES -
This is a tool that truely needs to be redesigned. It was originally made to be used as a curved skew for spindle turning where we are riding the bevel and all of the cutting forces are straight back into the handle; and there is very little bending force at the tang. Any use that puts a bending force on the tool can cause a problem and using a less ductile alloy for the tool only increases the problem because then it will break, rather than bend, at the tang. The larger this tool is made the worse the problem becomes because the thickness at the tang remains the same.
The modification of adding a piece of brass rod across the tank is a good one. Besides being a stiffer tool, the added weight is a benefit. It doesn't even have to be brazed in place to be beneficial. Bedding it into the tool with a flexible epoxy works as well as brazing. I have always wondered why some tool manufacturer hasn't started making them. I used to make this modification to the tools. It seemed like a good way to make a couple dollars, but I had to give up because I couldn't charge enough to compensate for the tool cost and the time required to modify it.
I see that P&N now makes a roughing gouge that is machined from a piece of round bar stock.
This message has become too long, but I hope that it will add something to the discussion.