ken chase

>I coated some roughed out bowls completely with anchorseal then placed in brown shopping bags sealed with tape to dry. Were the bags necessary since the bowls were sealed?

Thanks

Re: new drying question

#2

Re: new drying question

Jim K in Trappe PA

>I coat the outside of the bowl with Anchorseal, wrap in newspaper, and store them upside down. This allows moisture to escape through the uncoated inside, but the newspaper slows down the drying. I've made about 20 bowls of various sizes with this method, and no cracking yet.

Re: new drying question

#3

Re: new drying question

John Lucas

>Ken I rough mine out, coat the endgrain portions with anchorseal and then just put them on the shelf. I've only lost a few this year and one was because I left it sitting on the lathe for a day and the sun came through the window and probably dried it too quickly. I think I can still save it but it's going to be to thin to be a really functional bowl for and 18" bowl.

Re: new drying question

#4

Re: new drying question

Norm Smith in Nova Scotia

>Hi Jim,

No, the bags were not necessary.

Norm

Re: new drying question

#5

Re: new drying question

Rick in Lincoln

>Ken, that's exactly what I do and I can count my losses on one hand. If nothing else, having the date and species on the bag helps me to remember what's inside. Lately though I've gone to DNA with equal success.

Re: new drying question

#6

Re: new drying question

ken chase

>Rick:

After you soak in alc do you still coat and bag?

Re: new drying question

#7

Re: new drying question

Greg Haugen of WI

>After I soak the bowls in the DNA at least over night or longer for big bowls I wrap the outside with brown paper from Grocery bags tape the rim up so the inside is open. Store upside down on a rack so air can get to the underside. Success? Yes. Failures, yes but I believe my fault by having one area too thick, etc. I'm also starting the anchorseal on end grain only and drying-in 6 months I'll let you know. Anchorseal the whole thing-I'm in WI it's not that dry here, it really slows down and I'm a tad impatient. So I'm hoping that the endgrain only will do the trick. Find the DNA article from Dave Smith.

Hope it helps.

Greg

Re: new drying question

#8

Re: new drying question

Rick in Lincoln

>Ken, I follow Dave Smiths directions to the letter. Rough out to a bit more than 10%. Soak for 2 hours minimum, remove and air dry for 1 hour, then wrap with a grocery sack up to and including the rim. Label the paper with species and date. Store rim down and wait. I don't have a minimum time yet for finishing, most of my DNA processed bowls are still on the shelf while I finish off my year old supply of anchorsealed and bagged supply of rough outs.