Jack Guzman from Maine

wood drying/checking

Jack Guzman from Maine

I use green hard maple for chair legs. I buy it by the log and process it by hand. I cut the log into just longer than the longest blank I will need for chair legs/parts. Then I rive it into roughly 2" blanks. Wider sometimes depending on final dimension needed. Next I turn these blanks into the biggest round I can get out of the blank. The next step is where my question comes in. I like to dry these rounds for a few days in my heated shop to allow some of the water to evaporate. I paint the ends with anchorseal. To make a leg I will cut to finish length after this drying period and turn a leg in the lathe leaving the tenon large. At this point I place the tenoned end in a hole in my kiln for drying. I dry this part completely. I got impatient recently and turned the leg after only one day drying. When I put it in the kiln it began checking . I took it out and air dried it a day and tried again,no checking. Why did this occur?

I have tried putting a round in the kiln to speed up drying and the whole piece checks and splits.

What I need to understand is what is the process that causes checking? What happens to the cells to make the wood crack? How can I accelerate drying without checking?

I should mention. My shop is heated to 60 deg.with a vented propane heater. The heater lowers the humidity in the shop noticeably.

Re: wood drying/checking

#2

Re: wood drying/checking

Larry Barrett

I have tried putting a round in the kiln to speed up drying and the whole piece checks and splits.

What I need to understand is what is the process that causes checking? What happens to the cells to make the wood crack?

A living tree contains both free and bound water. When you buy a log and split it into billets, each billet will still contain free and bound water. Free water is not connected to the wood fibers in any way, either physically or chemically. It will evaporate/drip out of the billet as quickly as possible. As it leaves, there is no change in the dimension of the wood. Bound water molecules are different. They are chemically bound to the cellulose polymers in the log/billet. If they are removed from the cellulose fibers, the fibers shrink.

The bound is a weak one (hydrogen bond, I think - Bill Tindall helped me out with this a couple of years ago). But even though they are bound to the cellulose, the moisture in the billet still seeks equilibrium with moisture in the surrounding air. (Exactly why this is the case is covered in third year chemistry class according to Bill; I did not get this far). When you put your 2" round in your kiln, the warm air in the kiln can hold much more moisture than the moisture in your shop; the water molecules near the surface of the round leave their hydrogen bond with the surface cellulose molecules. The water molecules in the interior of the round will migrate toward the surface, but not fast enough to replace those that left. The cellulose fibers near the surface shrink and eventually pull apart.

I do essentially the same thing when making post and rung chairs. But my rungs are much smaller, about 3/4" octagons when I place them in my kiln. I run mine at about 120 degrees F. The rungs go in at around 20% MC and I take them out when they are bone dry. Because they are much smaller, I do not see any checking. You did not say what the temperature is in your kiln. If you lower the temp in your kiln I suspect you will not have a problem, or as much of one. I do not have any suggestions for drying your rounds any faster.

Re: wood drying/checking

#3

Re: wood drying/checking

Philip F Duffy

What a great response, Larry. Thanks! P.

Re: wood drying/checking

#4

Jack Guzman from Maine

140 deg

Jack Guzman from Maine

I think I'll have to read it a few times to understand everything you said but I got the gist. You answered me perfectly. Thanks Larry.

I set my kiln at 140. I used to run it at 120 but I do alot of steam bending and I need the higher temp to "set" the bends. I was getting some spring back at 120.

Re: wood drying/checking

#5

Re: wood drying/checking

Don Stephan

Regarding the impatient blank that checked in the kiln, then the checks went away . . . The checks are fractures in the wood, that might seem to go away when the moisture level in the end of the blank goes up. That dry wood undergoes an increase in moisture content as moisture moves from humid air into the end of the blank, moisture from the interior of the blank moves out to the end of the blank, or both. The fractures are still present, just not visible after the moisture content increased and the wood expanded slightly. It may not be possible to speed up your process without getting drying checks.

Re: wood drying/checking

#6

Re: wood drying/checking

Tony Wilkins

One thing i’ve Heard, I remember not where, was that it has something to do with the differential drying between the ends (open to the environment) and the middle of the board where drying is slower. Obviously the quicker you dry the more this would be the case, if what I remember is true. That’s why sealing the end grain is practiced.

Re: wood drying/checking

#7

Re: wood drying/checking

Steve Voigt

"How can I accelerate drying without checking?"

You can't. Checking happens when the wood dries too fast.

When you dry the wood too fast, all sorts of bad stuff can happen. There may be checks that you don't see, but the customer gets to experience them weeks or months later. The wood for sure will be more prone to warping, at least until it reaches equilibrium again. My advice is to slow down and be patient. I am just dipping into some beech that's been drying for three years. Wood dries on its own schedule.

Re: wood drying/checking

#8

Re: wood drying/checking

david weaver

Unfortunately, I think if you want to speed up the process of drying, you have to add pressure and temperature at the same time.

I see Steve answered. He and I probably have a pretty grim view of the world of drying lumber because beech will check on you with unsealed ends even if it's already fully dry and several years old. I've had long dry lumber check on the sides a few times, too - thankfully not deep enough to cause discarding expensive plane billets.

Horizon lumber (my interpretation) has tried various times to speed up their drying process with beech, and often paid the price (honey combing, etc). Even so, I think they still started with a substantial air dry period.

Re: wood drying/checking

#9

Jack Guzman from Maine

Re: wood drying/checking

Jack Guzman from Maine

I can live with waiting. I just was looking for a clearer understanding of the physics of it so I would know better how to improve my process. I will continue tweaking things til I'm satisfied. If I learn anything in the process I will share it here.

Re: wood drying/checking

#10

Re: wood drying/checking

Warren in Lancaster, PA

The wood shrinks as it dries. If the wood dries rapidly you will have it relatively dry on the outside while still quite wet on the inside. The inside is still swollen but the outside shrinks and is stretched and cracks. So you want it to dry slowly so there is not such a great difference between inside and out. Keeping the timber out of the sun and the wind and out of heated spaces is helpful for slow and steady drying.

The moisture generally exits the end grain faster than the side grain. This presents another special problem. The cross section at the very end shrinks and is much smaller than just a bit away from the end so end checking occurs. Usually we just discard the very end of the timber, but for valuable stuff we sometimes coat the end to keep it drying evenly with the rest of the piece.

Rough turning green removes the outside and makes the piece slightly smaller in cross section so drying can go slightly faster.

Re: wood drying/checking

#11

Turning green

Warren in Lancaster, PA

Turning a green blank for a chair leg (a cylinder) is helpful; it reduces the bulk of the billet and hastens drying. In historical times roughing out a wet blank was faster than roughing a dry blank. However turning a Windsor chair leg green exposes end grain in many places and makes these areas vulnerable to more rapid drying and end checking.

Re: wood drying/checking

#12

Jack Guzman from Maine

Re: Turning green

Jack Guzman from Maine

It's a juggling act. I have to be patient and do everything in a particular order allowing time for proper drying.

Re: wood drying/checking

#13

Re: Turning green

Barry Irby

My understanding of this is you turn the legs green (swollen) and the rungs very dry (shrunken) so that wen you drill the hole for the tenon, the tenon swells and the hole/mortise shrinks, it becomes very tight. And who ever assembled the chair (bodger?) even paid attention to the grain orientation to enhance the fit.

I'm guessing you already knew that.

My friend who made chairs had a box of sand with a heater under it and he inserted the tenons into it to shrink them as much as possible and then inserted them. I think he put them back on the lathe after they were fully dried and still hot and re cut the tenon with a wrench he had sharpened for the purpose of cutting a very exact tenon. His chairs held up well.

Re: wood drying/checking

#14

Jack Guzman from Maine

Re: Turning green

Jack Guzman from Maine

I used sand for awhile at first. I put a pan of sand on an electric hotplate. Once I built my kiln,all I had to do is drill holes in the top of the kiln and I set the tenon end of the legs in these holes.