Two things from today.

I started to varnish the cherry telecaster body with epiphanes, just rubbing it in with fingertips rather than brushing on a heavy coat. If it dries OK, I think I could get along with it without ever making varnish - but it stinks!! and if you rub it on with fingertips only, you won't be washing it off - turps to the rescue. So, gloves from now on, because I'm sure it's full of stuff you shouldn't absorb.

I also made a batch of pine and dammar resin and linseed oil varnish.

There is a video on youtube of the process, so I followed it. Nothing special, just copied the method, though my electric hot plate had trouble approaching 300C.

The picture is the jar of varnish straining slowly through microfiber. I don't have any paint strainers in the house, so the slow microfiber cloth will be the way.

The process itself was pretty easy, though there is a dangerous period when you combine the oils and resins, the whole mix bubbles way up (and if I was at higher temperatures, I'd figure it would do it very quickly). Absolutely not a process you would ever do in the house no matter what (the smoke from burning the BLO and then the smoke from the final part of the varnish making is pleasant smelling, but I'm sure it's bad for you because it's past the smokepoint of everything in the mix).

George told me that he's had mushroom clouds making finishes when they bubbled over, and watching the oil and resin mix go off into a foam before it settled makes me certain I never want to do this over an open flame (not because of danger, which is certainly present, but because I'd be afraid of losing the batch).

Anyway, I covered the mix at the end out of desperation, and it got up to about 290C and then quickly passed the string test (which is confirmation that the oils and resins have bonded).

When finished, I believe it will fill the quart jar about 1/3rd full, and I think the final cost per batch with good ingredients (turps that smell like pine, food grade flax oil) will be about $30-$35. To brush this, it needs to be thinned further with 1 to 1 turps, so you get about 2/3rds of a quart of brushable varnish for about $55 (a pint of turps from europe is about $20 - the US suppliers are $35 or so). It doesn't stink at all like the commercial stuff does, and apparently there is some sort of homeopathic movement that uses turps in a bath so there is a supply. No thanks on using it for personal care, though!

George suggested japan drier, but very little - only a drop or two or the varnish will overharden and crack - if it has trouble drying. It shouldn't if it passes the string test - which is letting a drop of the batch cool on a stable surface and then putting your finger in it and then pulling away and seeing how long of a string you can form before the string breaks. 5cm is the threshhold from the video.


Re: First batch of varnish

#2

Re: First batch of varnish

david weaver

Guitar with light coats of epifanes.

Two coats. Lots of ugly stuff on the cherry on this guitar, but it'll all be covered, as will my poor routing. As dumb as it sounds, I don't do a lot with a router, or power tools in general, so I had some trouble with the template and didn't know the bearing wasn't on it.

I also pulled an eighth radius bit out for the top of the guitar, which is correct for a telecaster, but forgot that I had it cutting overdeep on my kitchen cabinet doors. The result is that I had to increase and flatten out the radius on the front of the guitar a lot and that's not really what I wanted.

All that said, the hardware will cover up all of it, so you won't be able to tell.

One rookie mistake on the neck (overcutting the pocket under the truss rod nut since I cut everything else on this other than the pockets by hand. Next time, I'll plow a groove straight through to the peghead and the'll be no need to cut low. I'll have to fill that spot in the back of the neck.).

As well as I can build a plane, I know that the first guitar will be a learning process and there's no need to stall on it, just get through it and see what to avoid next time (I'm building a second one with expensive hardware).

https://s15.postimg.cc/it0rbkw17/20180805_123155.jpg

I wasn't going to put varnish on this junker, but I'm glad I did. I've learned that from now on, I'll be diluting the varnish and applying it with a rag. The two finger method like you'd do with a violin, varnish unthinned, works fine, but it won't make a coat that's particularly even.

Two hours in the sun for epifanes is worth a day inside, it cures quickly outside.

Re: First batch of varnish

#3

First batch curing report

david weaver

The varnish was really slow to cure -my varnish, not epifanes.

Then I went to violinvarnish and saw that for an amber varnish of this type ("one of the oldest types, or something like that according to the listing") the seller says UV light is needed for a cure less than two weeks.

So I put eipfanes and this on a test piece, and both were suitably dry in the sun in about 4 hours. The seller of this type of varnish said 13 hours in the sun for full cure.

I also saw that my price comments were not for this type of varnish. For this type of amber violin varnish, the seller wants $72 for 100ml (!)

Mine turned out much thicker than epifanes, so I thinned it with turps in the jar after seeing that it cured. It's almost too thin with less than a 1 to 1 ratio, but it'll work well for wiping. it feels like a heavy cut of shellac now, except you can play with it for a while when applying it because it doesn't set quickly.

I don't know that most of you guys on here will ever do this, but it's fun to make a finish and then see it cure properly. it smells wonderful. I know that the pine turps is still toxic and shouldn't be breathed, but it makes the shop smell like pine. The epifanes is not so pleasant, but it's sure cheaper. And the way it goes on and sets up quickly, I can tell it's intended for outdoor use like a spar varnish. I will thin it with its brushing thinner before using more of it.

Talking to george yesterday (and if anyone asks, I see people are concerned because he's not posting on forums, he's actually fine - I think he's just lost interest in the forums) - he said stradivari liked to hang his violins in the sun on a cupola to get them to cure, and it was the king of spain he had to apologize for sending a pair of violins that had varnish that never cured.

This just goes down as another thing where I remember seeing people talking about it ("cooking varnish") and thought "I'll never do that, that's nutty", but by a stroke of luck or perhaps just following instructions, the first batch is good, and the next batch won't cost so much to make.

Re: First batch of varnish

#4

I look forward to your youtube video.


Re: First batch of varnish

#5

Re: I look forward to your youtube video.

david weaver

Sorry if I made it sound as if I'd made a video of the process. I didn't, it's largely an elapsed time process where you do something else and come back and check it from time to time until the point when you mix the oil and resin (both turn to a foam together and expand before they settle).

this is the video that I followed:

https://www.youtube.com/watch?v=gh5JTATnl4k&t=341s

Mine came out quite a bit darker, but I think it's because I struggled to get the burner to heat the mixture to 300C for so long, and it cooked for a long time at about 250C before I covered it.