Re: Hardwood floor expansion
Sgian Dubh
>American Ash has tangential shrinkage value of about ~7.8% and a radial shrinkage factor of ~4.5% from 30%MC to 0%MC.
If your boards are currently 15%MC and they stand a chance of drying to 7%MC when laid out as a floor in your house then you can expect a 36" wide cross sectional assembly to shrink by anything up to 3/4" at some point within the next twelve months.
This is a worst case scenario assuming every board is perfectly tangentially cut, ie, there isn't any rift or quarter sawn parts in any of the boards which means they would shrink less across their width. I'm also guessing at the current MC being 15%; it could be less or more. And it's not absolutely certain a floor in a house will dry to 7%MC, but it's possible.
So I've provided you with what could be pretty close to the maximum shrinkage you might expect. It would be prudent to let the boards acclimatise to current indoor conditions for a couple of weeks if you don't know what the current MC of the wood is.
Why not stick a moisture meter into the stuff and get a reading, then decide what to do? If the wood currently reads about 9%MC or 10%MC go ahead and do the floor. If it reads 15- 16%MC I'd let the stuff acclimatise for a couple of weeks. Slainte.