Spring back revisited and glue learnings
Bill Tindall, E.Tn.
The assembly is out of the clamps..... a second time...... and I learned something.
There are two important considerations. The yellow Titebond glue has a crosslinking additive that is reversible with water and/or heat. This additive will not fully function to provide a rigid bond until the joint is dry. When a lamination is assembled a ton of water is added to the wood from all the glue joints. It is known that a panel edge joint can take days to cure to full strength if the lumber is high in moisture content. With these facts in mind....
After 24 hours I took the lamination from the clamps. During this cure there was a layer of glue resistant and moisture impervious tape on the bending form and a caul on the other side. In retrospect, the only route for water to escape was through the edges and I doubt much escaped. When released there was 1/2" of spring back and it was not uniform along the curve.
I removed the caul, added back a few clamps to anchor the lamination to the form and put the assembly into a car.
Cars are wonderful solar heaters. In the winter I cure finishes in the back of a Ford Explorer. In the summer they make good solar kilns.
After an additional 2 day bake I removed the lamination from car and clamps. The bend was now uniform with a slightly less than 1/4" spring back, precisely what was calculated from the formula provided in a previous post.
The moral of this story is that yellow glue won't set to full strength and rigidity, and lack of creepiness, if drying is hindered in a bent lamination assembly involving cauls, wax paper, packaging tape, etc.
As others have pointed out there are adhesives that don't involve water and others whose rigidity is less affected by moisture in the wood. If you don't happen to use these and instead use Titebond, lamination drying must be considered.