I would like to add a couple things to the fine advice given above re: reading the Lee Valley instructions.
A. The moisture content of the wood to be bent is a fundamental factor. Be sure to stay within the guidelines recommended in the Lee Valley pamphlet. About 15% to 20% as I recall. My experience has been the closer to 20% the better.
B. The recommendation is to steam articles about 1 hour for each 1" of thickness. My experience is that a little longer is better. Perhaps 1 hour 15 minutes per inch of thickness.
C. If the articles will be bent to subtle curves, then it is not necessary to use a steel band to put compressive force on them during bending. However, if the bends will approach or exceed a 90 degree angle, then I strongly recommend the purchase of the steel band compression kit offered by Lee Valley. You risk blowing out the grain on the outside of tight curves if the article is not under compression during the bend.
D. Be sure to have a strong template that the article can be formed to after the bending. Have plenty of strong clamps set up to the right sizes ready to go.
E. After the initial bending, my experience is that the articles should remain clamped to a template for a period of a couple months to allow them to fully dry adhering to the desired shape. Early removal from the template risks springback, distorting the final shape.
Hope this is useful.