I have a trailer load of mostly poplar sitting in my driveway. I had it sawn a few months ago. Its stickered on the trailer and sitting in the sun. I know the rule of thumb is to let it dry for a year per inch, but can I start using it sooner? I have a small moisture meter. If I meter it and its dry does the year part make any difference?
I'm considering using it for "white" wood (internal parts) in furniture. Also things like closet shelves. How about if I plane some of it and bring it into the air conditioned house?
I think you are going to need some elevated temps if you want to use it soon. Just sitting around isn't going to speed it up, and sitting around in 70-75 degree house isn't much better, despite the a/c. Now if you build a rigid insulation box, add a couple light bulbs, and throw in a dehumidifier, then the moisture will drop quickly.
I did that once, with an end table I made for my daughter. I thought the wood for the drawer sides was dry, but with the first humid weather that hit, those sides swelled to the point where I had to use a Stanley Wonder Bar to crank out the drawer so I could plane it down.
If you use it, I'd allow a bit of leeway in your final dimensions. I definitely wouldn't use it for any wide part.
We use a bit of air dried wood around here. My different friends have different methods of getting to the end result.
If there has been an air flow over the wood to draw off the "humid" air then the wood dries a lot faster than just sitting around "stickered" - no matter how warm it has been. Light bulbs, vent fans, sun - all achieve similar results. Air flow is the important thing.
I have one friend who stores his wood in his attic and relies on the heat of the attic to dry his wood. His attic has the ridge vents so there is always a flow of air from the soffit vents to the ridge vent.
I've used a "heater box" with light bulbs and vents top and bottom. But that only works for smaller pieces.
Jim uses his solar kiln - which works quite nicely.
I know it has been a bit warm - but if you haven't had the air flow - I don't know if I would chance it. You can always try cutting a board a foot or so into the board and measuring the moisture on the inside. If the moisture content is reasonable - then it will probably work.
What MC would you use as a starting point? If the wood is dry, how dry is dry enough?
Does TIME have anything to do with it? that is, does sitting for a year make the wood better than drying it quickly? Is there some kind of internal chemistry going on? (I am guessing not because most lumber is commercially kiln dried and they are not letting it sit for a year.)
So, I have a greenhouse/solar kiln. Should I shove some of it in there and let it cook? this is a daunting task. The space is already jambed with other wood and the load of lumber has 12" wide 17' long pieces on top that I can't reach and are too long to go into the kiln. So, I guess its time to get up there and drag em down and cut them up and stuff them into the kiln. Nothing happens until I make it happen.
Drying outside will usually get you to about 15% MC [in your location]. That's not good for interior use. The wood needs to reach stable EMC (equalized moisture content) meaning the entire board needs to meter at the same MC and be consistent with the old wood in your home. You can find that value easily by putting your meter on a solid piece of wood in your house, even a framing member, because all wood, regardless of variety, will reach the same EMC in a given location.
The one year rule presumes that the wood has gone through a full range of seasonal expansion and contraction to reach equilibrium.
If you wish, you can move your stack inside because that will speed things up a bit, especially if your house is air conditioned which works as a dehumidifier. You should have the wood sit in your shop, stacked and stickered, for a week or two anyway before using it to let it adjust.
that year per inch is not so. That got started a long time ago. Wood i have cut has dryed earler than tnat. I stand my wood on end's. I don't stack it flat. The mooister goes to the bottom of the wood faster due to the gravety. The old timer's done it that way. Used to hang it up like you would hang meet up in a coolor. If it has been their that long i bet it is dry enough to use. I guess no moister meter? Good luck also this Joe, do yourself a favor and pick up a copy of Dr. Gene Wengert's "Drying Hardwood Lumber". There is much more to drying than can be covered in a few paragraphs.
Drying rates vary depending upon species and thickness. The "1 year per inch" rule is not accurate.
You can easily damage the wood during the drying process, and too much airflow (above 350 fpm or so) will probably damage it, at least in the early drying stages (above 35% MC).
Your miller needs to either treat the ends of the logs with a high quality end sealer (such as Anchor Seal Classic) before transporting them, or plan on cutting off 5" or so of the ends of the logs after transport and before milling. The reason why is the airflow past the ends of the logs will be in excess of 5300 fpm during the trip from WVA to GA - well in excess of 350 fpm! The checking that starts during this time will continue on through your boards, much as a crack in glass will extend itself.
Also do a search on the archives here for drying related info.
Time certainly has something to do with it. The year is a rule of thumb assuming changing weather conditions, temp, relative humidity, etc. Sure doesn't take a year in the Arizona desert The one year is kind of a sure thing if you don't have a meter. You can use your meter instead of a time limit. You can also hammer in a couple of nails and use those as pin extensions to get a more accurate reading deep in the board - surface will be more dry if the board hasn't yet reached equilibrium .
For what do you want to use the wood early? Might be ok for shelving or something where shrinkage will not cause major problems, though it might also warp too much. Using less than dry wood is a gamble, no two ways about it. I've seen it work and I've seen disasters.
Commercial lumber is dried to a target of 7%. In fact it is usually dried to less than this amount and then steamed back to 7% to relax stress.
For most furniture purposes I would want the wood less than 10%. I see little reasons to dry it all at once. Move what you intend to used in the next year into the green house, add some fans and in 3 days it will be dry if it is poplar.
Hi Mark, To answer a couple of your questions (bear in mind I an not an expert), I use a lot of air dried wood - some of which is probably 50 years old other less than 3 years. I purchased a decent Moisture meter a few years ago. I store all my wood in my shop, most of it upstairs. I tested the wood inside my house (door casings, trim) in an inconspicuous spot (I have a pin type meter). In my heated air conditioned house I found the wood to be 6% or under. So as a general rule I won't use anything over 8% for furniture. However the kiln dried wood I purchase from my sawmill is stored after drying in an unheated warehouse so may be above that when purchased. I usually leave it in the shop for a couple of weeks if using for house inside trim. For furniture use I leave it at least a month - then test it to be sure it has equalized to under 8%. I have had some warp when used too early. Every thing I have stored upstairs in my shop which is kept heated and air conditioned is down to less than 6% after a year. Most of the lumber I have came from Amish / old order estate sales and most of it was stickered and air dried - stored in buildings when I purchased it. As to your question about kiln VS air drying - all woods can be done either way with fine results. When air drying the wood must be stickered and enough air flow / heat etc applied to dry fast enough to prevent fungus/mold yet not dry the surfaces so fast that the center is not allowed to release the moisture at the same time. If dried to fast the wood will "check" and/or crack/split. Kiln drying is done in the same way on a ridged schedule to prevent the same issues. To further complicate the issue there is a vast difference in the amount of care you must take with various species. White Oak is very difficult to kiln dry properly. Too fast and you get massive checking and "case hardening". Other species like walnut, cherry & Ash are far more forgiving. There is also a vast difference in the actual moisture content of fresh cut wood - Ash is around 50% (half water) while cotton wood is around 150% (more water than wood weight). To me the price of wood is small VS the time I spend building something (and the cost of finishing material, equipment etc.). So I won't take any chances on using incompletely dried wood that may shrink or warp.
The higher temps of kiln drying, 130 degrees for several hours, will kill any insects and eggs in the wood. See all the questions about powder post beetles.