Re: Issues with CrystaLac grain filler?
Mark Mandell - Gone Round In Jersey
Hi Doug,
I've used it for years to do filled pore finishes on walnut; haven't had any problems. My routine goes like this:
1. Sand the surface to 180 and vacuum off well.
2. Apply a spit coat 3/4 lb cut of dewaxed shellac; let dry for 2 hours.
3. Apply a first coat of Crystalac filler and work into the pore with a plastic straight-edge going first with, then at an angle to, the grain. The "squeegee" will remove the excess. Allow to dry 2 hours.
4. Resand with 220 paper.
5. Apply a second coat of filler, going lightly with the squeegee to leave more filler on the surface. Allow to dry well (2-3 hours).
6. Resand with your final grit paper on a flat wood block moving with the grain. I find that a power sander's platen surface tends to flex too much for a truly flat surface. The dried filler sands easily, so this isn't the chore that it might sound like. Shaped edges and molding profiles can, of course, be a pain.
7. Apply your finish. I've used shellac, NC lacquer, oil poly, and good waterbornes over Crystalac with no issues. Remember, however, that any waterborne finish applied to a raw-sanded surface will tend to raise the exposed wood fibers. Perhaps this is what people read as the filler shrinking. Another spit-coat of shellac before application of a waterborne finish usually solves this problem for me.