A friend of mine has contracted me to refinish a large, cherry veneer dining table. The original finish had some round water marks and he tried to use some unknown "furniture finish rejuvenator" on it that made the original finish worse than it probably was. Sanding just gummed up the sandpaper, so I have used a cabinet scraper to remove most of the finish. Because the veneer is so thin, I am looking for suggestions on final preparation and finish. I plan to use Target Coatings Waterbase Poly over some sort of natural cherry stain, but any info or suggestions are appreciated.

Re: Refinishing cherry veneer

#2

Re: Refinishing cherry veneer

Dick Coers

Cherry isn't as bad as many woods, but refinishing always brings up the subject of contamination. Materials left in the pores of the wood, consumer wax products, etc......I would contact the clear coat supplier and talk about acceptable barrier coatings. Shellac was always the universal, and I suppose dewaxed should be acceptable for the water based, but I would get their recommendation. I always lay on the first couple of coats, on any refinish job, pretty dry. Heavy coats of clear present more trouble grabbing on old wood, versus lighter, drier coats.

Re: Refinishing cherry veneer

#3

Re: Refinishing cherry veneer

Mark Mandell - Gone Round In Jersey

Chuck, can you be a little more precise as to what "most" is in your view?

Cherry's tendency to splotch due to the fruitwood compression issue makes it hard to tell you where to go with this without the piece in front of me. I suggest the your wet the entire surface with either de-nat alcohol or naptha to see if there is still some of the film finish present (it will show up as lighter patches where the liquid doesn't soak in a bit. Take your scraper (wise choice) back to any spots revealed.

Once you are confident that all film finish is removed, you can choose to color with a stain (oil or NGR only) or, if you've got serious color differences, a 2-part bleach application, followed by stain.

Once coloring is done and even, make a thin application of fresh dewaxed shellac to seal the colorant (oil or otherwise) to prevent its leaching into the waterborne. Since you will be using Target (great stuff) know that they strongly recommend nothing older than 3 months including SealCoat when sealing with shellac. The shellac tie coat must be thin (no more the 2 light coats) and freshly mixed/made to avoid cold checking under the waterborne.

Lastly, give the piece at least 3 days to fully evaporate the sealer solvents before applying the Target. This prevents lingering solvents from messing with the Target chemistry.