Vacuum pressing photos
Grant in Iowa
A while back we were discussing the benefits and problems with vacuum pressing. I thought I'd share some photos of a part that just came out of the vacuum press this morning. I am making laminate bent water skis with Formica for the outside layers. There are 4 layers of Ash, and two layers of Formica on this part.
The first photo below is of the part fresh out of the press. I use Dap Weldwood acrylic resin and let it set up in the press overnight at 75 degrees and 26" of mercury on the press. The waxed paper I use to protect the bag and form from glue squeezeout is still on the part in this photo. When I am preparing the part to be placed in the bag, I use blue painters tape to hold the freshly glued layers of the sandwich in alignment and in the right place on the form.
Here's a shot of the blank with the waxed paper removed. This is #1, and I began to worry about starved joints when I saw the lack of glue squeezeout. I used a foam roller to apply the glue between the layers. I am not seeing any evidence of starved joints yet, but I will apply more glue to the next parts to be sure.

The process of shaping the part from this point goes like this. I make and perfect a template of 1/4" masonite of the outline of the ski. I lay and clamp this template over the newly formed blank and trace its outline on the concave side of the ski. I remove the template and cut the shape close to the line at the bandsaw. I reinstall the template with clamps and, using a bearing guided bit in a router, follow the template to create a part that perfectly matches the template. With a roundover bit, I slightly round the edges. Here's what it looks like after that process. All it needs is the edge lightly sanded and finished, and the hardware applied:

The real point of my post is to share the quality of the glueup using the vacuum press. Nice, fine gluelines, nearing the quality of baltic birch ply. Dap wants a glue thickness of .003" to .006" for best results. I started with a total material thickness of .730", and finished with a thickness of .750"... or about .004" per glueline. Right in the butter zone. I built a prototype ski last summer and it has held up well so far with similar glueline thickness.
Here's a couple shots of the edge and rear or the ski so you can see the gluelines (as well as my camera and photography skills allow, that is):


In the "If I had it to do over" category, (and I do, I have to make several more), I'd add a layer of hardboard between the part and the form in order to protect the form a bit.
Hope this provides some insight into the value of vacuum pressing when doing laminate bends, I know there was significant interest in the subject last time it came up.
Regards,
Grant in Iowa