Re: Precat lacquer finish problem?
Sgian Dubh
>How many coats did you apply, and how thick was each coat? That may point to the problem.
If you didn't apply as follows that could be the cause.
Pre-cat lacquer should be applied at about 100 microns per wet coat which, when fully cured and the solvents have evaporated, leaves a dry film of approximately 50 microns. Total dry film thickness should be no more than 150 microns. This therefore allows you to put on three coats at 100 microns each. Note: 100 microns is about the thickness of a head hair.
You can also apply two wet coats at about 125 microns per coat leaving a dry film thickness of about 125 microns.
Dry film thicknesses exceeding 150 microns are liable to cracking, usually across the grain, but sometimes with the grain, and in the worst cases it looks like 'Chinese writing'. This is because the finish is relatively brittle and as the upper surface flexes somewhat out of sync with the rest of the film below, stresses build up leading to the cracking. The fault usually appears weeks or months after application, and sometimes grain movement below the film increases the tendency of the film to crack, and in this case my experience is the cracking is more likely to follow the grain. Slainte.