Staining and finishing QS oak

Larry Chasteen

>I've read about 1000 articles and all I've accomplished is confusing myself. I've built a QS Oak desk. I want to darked, fill the pores and apply some sort of finish. Should I stain, seal sanding sealer, fill the pores with a neutral or darker filler (I haven't made up my mind which way to go yet), seal again with sealer to lock in the filler and then finish with poly?

Re: Staining and finishing QS oak

#2

Re: Staining and finishing QS oak

Hank Knight

>Larry,

Everybody has their own recepie for finishing oak, so you'll proably get a lot of differnet responses. I'll give you mine:

I add Transtint dye to Behlen's water based wood filler. I use a combination of Dark Mission Brown and Medium Brown Transtint. I find the Dark Mission Brown too dark for my taste; the Medium brown lightens it up a little. Try different dye proportions on sample pieces of your oak to get a color you like before applying it to your piece. The more dye you add to your filler, the more intense the finished color of your piece will be.

Apply the dyed filler according to the directions on the can. Be careful, it dries real fast; and if you put it on too thick, you'll have a lot of sanding to do to level it. When you do sand it level, you'll find that the filler fills the pores in the oak with a nice neutral color that doesn't stand out and the dye darkens the oak significantly. Some oak finishes highlight the grain of the wood and give the piece a raw appearance I don't care for. This method doesn't highlight the oak grain. Instead it gives you a nice mellow brown that you can regulate with the Transtint mix, but it allows the medullary rays of QSWO to show. Seal it with a coat or two of SealCoat shellac and apply your favorite finish. On heavily used pieces, I've had good luck with wipe-on poly. I use 5 or 6 coats of gloss. After the last coat, I knock the sheen off with wax applied with 0000 steel wool and buffed.

My $02.

Hank

Re: Staining and finishing QS oak

#3

Re: Staining and finishing QS oak

Fred Davis

>Fumed Oak is very attractive and can be done simply by putting a plastic tent over the desk and set a few dishes of Ammonia inside check it for color every hour or so.

Nearly fool proof way to color Oak.

FredD

Re: Staining and finishing QS oak

#4

Ellis Walentine

There was just a thread yesterday... *LINK*

Ellis Walentine

>... about recreating a Stickley finish. Jeff Jewitt has some very simple and straightforward recipes on his website. Go check it out.

Ellis Walentine, Host


Jeff's site

Re: Staining and finishing QS oak

#5

Re: Staining and finishing QS oak

Jim Hoeller------WebKitFormBoundarycQB+IfmNjFaVxeA

>Fuming oak (white or red) requires the kind of ammonia sold by blue print supply houses. It is full strength and highly toxic. Do not use it in the house or any enclosed room or garage. A carport or very well ventilated covered porch is acceptable. The varieties of ammonia sold at supermarkets are not strong enough to work in a reasonable amount of time. I have used pvc pipe for the frame of the polyethlyene tent and lots of duct tape to seal it. A discarded processed food tray makes a good container for the amonia. Leave a small access port on the tent, pour the amount of ammonia needed (just guess), put the container in the tent on the bottom and seal the tent. Check the desk every couple of hours but don't open the tent. It may take 24 hours to achieve the desired color so be patient. When done, the desk will have a dark brown color with a grayish cast; don't panic, it will go away when the desk gets a light sanding and is varnished. The color goes deep so sanding edges a bit too much will not affect the color.

Re: Staining and finishing QS oak

#6

Ammonia

mdclor

>Normally, industrial strength is suggested, but I have fumed pieces with regular household ammonia and it has worked well.

Re: Staining and finishing QS oak

#7

Respectfully,I disagree

Andy Lincoln,in Dearborn,MI

>I think household ammonia works just fine.It may not be as quick as blueprint ammonia but it is alot cheaper and easier to get.I have lived in the same area of Metro Detroit my entire life,work inth econstruction industry and currently cannot think of a place that sells blueprint supplies.I am sure they are there but I just go to my local grocery store and buy ammonia there.

Here is a pic of some QSWO that was fumed for less than 8hrs with household ammonia.On the right lower corner is a coat of Waterlox wiping varnish applied just before the photo was taken.

From Recent work

And the project completed looks like this:

From Recent work

Andy

Re: Staining and finishing QS oak

#8

Re: Respectfully,I disagree

Fred Davis

>Andy ,your right , I have similar results with household Ammonia , blue print ammonia is really strong and not necessary, but will work .

Just painting Ammonia on the Oak will give you some color, though the wood will smell then.

FredD

Re: Staining and finishing QS oak

#9

Re: Respectfully,I disagree

Howard Norman

>Andy, you are correct. Household ammonia will work just fine. It will just take longer, that is the only downside that I can think of. The large chemical distributors, like Ashland and VW&R, will have the higher strength ammonia but if they will sell it to you is another matter.

Re: Staining and finishing QS oak

#10

color fastness?

Bill Tindall, E.TN

>I tested color fastness of ammonia-fumed mahogany and it was not nearly as light fast as the water soluble dye stains on mahogany. What has been the experience with oak if the finished piece is in a sunny room?

Re: Staining and finishing QS oak

#11

Re: Ammonia

Dave Bair, Eaton Rapids, MI

>I agree; it may take 36-48 hours, but household-strength ammonia will work. I just finished two Stickley plant stands and can confirm this.

Re: Staining and finishing QS oak

#12

Rick L

Re: Fuming white oak...

Rick L

>is typical. Red oak in another story. It doesn't have the tannins that white oak does so it dosen't fume well. We cheat by brushing on a mixture of tannic acid and water. Tannic acid is a powder. The moisture speeds up the fuming process as well. We routinely do timbers for timber framing and use anhydrous ammonia. You can't get ammonia any stronger than that. Regular household ammonia will work fine for fuming. It just takes longer.

Re: Staining and finishing QS oak

#13

Re: color fastness?

Fred Davis

>I dye Mahogany, since the Cuba stock is unavailable . do I can't relate to fuming Mahogany.

What I know about sunlight is fairly simple , direct exposure will damage the finish eventually regardless of the finish with the possible exception of paint.

A "sunny room" with the light level constantly even around the piece , the color change may never be noticed since it would be relatively slow.

For our own Furniture , we keep it in indirect lighting as much as possible.

For a startling example , check a Table with extension leaves that had not be been in the light of day , against the Table color, if the Table had not been covered with a cloth or pad.