Re: Spraying WB Lacquer
Mark Mandell - Gone Round In Jersey
>Hi Howard,
Few more things you should know about waterbornes and spraying them.
Waterborne finishes are very INtolerant of surface contaminants like oil and the stearating compounds used in most treated sandpapers. If you use stearated paper to sand your piece, or stain (water or oil), you will usually need to seal the wood under a tie coatbefore applying the waterborne. Water-dissolved dye stains will leach into a waterborne coating unless they are sealed first, and oil stains can present some adhesion issues if not fully cured. Best for this (IMHO) is a coat of 100% dewaxed shellac. The shellac must, however be fresh. If you mix your own shellac from flakes, do not use it under a waterborne finish after 90 days unless it's been refrigerated, and never after more than 6 months. Jeff Weiss (Target Coatings' owner) informed me of this problem (applies to other waterbornes as well). Personally, I mix small fresh batches of shellac for each finishing job. Using old and/or thick shellac coats under these new finishes can often lead to "cold checking" where the shellac literally cracks under the waterborne coating. If you use Zinsers' SealCoat (good stuff), check the 'borne-on' date and reject if older than 1 year.
A shellac sealer will also prevent the waterborne from raising the wood grain as was mentioned. You can use a sanding sealer, but make sure it is compatible with the top coat. Whether shellac or other tie/sealer coat, be sure to give the application 24 hours to fully dry and evaporate any primary or tail solvents before you begin to topcoat.
HVLP guns were (mostly) invented to apply waterbornes. Make sure that your gun is set up with the proper cap and needle. While a .8 or 1.0 cap will apply shellac or NC, you may have trouble with a higher solids waterborne. I've put Target's USL down like glass off-the-gun with a 1.2 cap. Remember, however, that you can't "thin" waterbornes like you do solvent finishes lest you mess up the chemistry balance. Target does make an additive, called SA-5, to assist with brush application of their own finishes, but you should plan on using their finish straight from the can (after straining, of course). Any questions on this score can be addressed to Jeff Weiss at Target here in New Jersey or Jeff Jewitt at Homesteadfinishing.com will give you excellent application how-toes.
If you're used to NC lacquer, spraying waterborne is a bit different in that you do NOT "double hit" the coating. I know some who push solvent lacquer with reapplications on short intervals. Do NOT do this with waterbornes. Allow a good two hours between coats or you risk sags and curing issues.
Waterbornes are now my exclusive topcoat, and I have been most pleased with their clarity and performance. Other nice thing is you won't need a very expensive explosion-proof fan to vent your finishing area as you would if using NC lacquer.