Dale Lenz

My lacquer finishing process

Dale Lenz

>I've been spraying lacquer for almost two years now. I use SW Cat lacquer. If I'm after a high sheen I do the following on something like cherry, tight grained wood.

Step 1: Put a sealer coat of 1# Seal coat. Thin lacquer about 15%, 85% lacquer, 15% thinner. Shoot four coats of lacquer( 10-15 minutes drying time between coats) wait at least two hours and sand down with 400 grit paper. Not uncommon to rub through the finish at this stage

Step 2: Shoot 4 more coats of lacquer on, wait at least two hours and sand down with 600 grit. Often will not rub through finish.

Step 3: Shoot 2 coats of 40% thinned lacquer, gives me a smooth finish. Wait 2.5 days or longer and work the lacquer by using 800 grit sand paper. Then I use several grits of automotive rubbing compounds with wool bonnet to get to the high sheen.

Question: If I'm not rubbing through the lacquer after step 2, could I not just wait 3 days and start the high sheen process. I have always assumed that Step 3 gives me a little bit of wiggle room, more surface finish, but then again it's more/extra work Maybe(?).

Re: My lacquer finishing process

#2

Re: My lacquer finishing process

Clint Searl, at the base of Haycock Mtn

>It may be different for a catalyzed finish, but the schedule I've used for 30 years for NC, CAB acrylic, and alkyd lacquers is much simpler and less laborious. All finishes are self sealing, and after trying a vinyl sealer that made no difference, I shoot the final from the start. Shoot-flash-shoot-etc with a 15-20% reduced mix till the build looks right. After it hardens off, mist shoot it with an almost straight reducer to even out the sheen and film. In a week or so it's ready for a rubout: 0000 steel wool and Butchers Wax to soften a gloss or auto polishing compound by hand or with a bonnet to deepen the gloss.

My current favorite for any wood is SW Alkyd Medium Rubbed Effect. It builds and levels great and hardly needs any rubout to produce a deep soft glow.

Clint

Re: My lacquer finishing process

#3

Re: My lacquer finishing process

Fred Davis

>While "all finishes are self sealing" is true to a degree, some are more water resistant then others, none that I know of are water proof over a extended period of time.

I used to use Nitrocellulose based Lacquer until CAB came along in a pre-catalyzed form.

All of the manufactures like Gem, Campbell etc., recommend Vinyl sealer under that finish.

I don't like it's sanding ease compared to Nitrocellulose based sealer , but it is the vinyl sealer that gives the finish the most water resistance.

You also can buy Vinyl pellets to add to Lacquer up to about ten per cent that will increase the water resistance.

Like Clint says , I think you could eliminate some of the hard work you put into your lacquer finishing.

I learned lacquer finishing from professional paint contractors who let very little grass grow under their feet.

All used sanding sealer , hand sanded with 220 garnet "A" weight paper.

Rarely if ever used more then two coats of sealer because to much makes the lacquer finish soft.

Kitchen cabinets got as much as four coats of finish (all used airless rigs as do I) with a high grade gun like a "Silver Graco" with a double stacked orifice that under clean conditions will give a finish slick as glass.

Sometimes if there is a little over spray , this will be handled by shooting with straight thinner, sometimes a slower one then the one you generally would use.

The Gem lacquer I currently use is applied straight from the five gallon container with no thinning as recommended by Gem. Sometimes I used "rubbed effect" and sometimes semi gloss.

For furniture, I take the process a step farther and go thru several different grades of Meguiars Auto Finish rubbing cream.

Hope this helps, it works for me.

FredD

Re: My lacquer finishing process

#4

Dale Lenz

Re: So...

Dale Lenz

>what I'm reading from Fred and Clint, neither one of you guys sand the finish down, correct?. Let the lacquer cure, then wool or compound your finish to the results you want. BTW a typo: I use CAB lacquer also.

Thanks for the past post

Re: My lacquer finishing process

#5

Re: So...

Fred Davis

>About the only time I will sand a lacquer finish is if I can see that going over it with 800 wet or dry wrapped around a cork block will even out the finish.

Rarely needed to do this , after I spent considerable time and money learning to spray with good equipment.

So, on kitchen cabinets for instance , I never need to touch the finish and women start comparing it to the furniture they have and wonder how come the cabinets are much smoother in most cases , depending what they are comparing it to.

If they have a house full of Baker furniture, then the process becomes more tedious. ;-))

FredD

Re: My lacquer finishing process

#6

Dale Lenz

Re: My lacquer finishing process

Dale Lenz

>I truly wish to thank Clint and Fred for their responses. Although, I never did get my original question answered. I think Fred and Clint might be speaking of a commercial lacquering application. Kinda of kin to a new car off the show room lot, nice paint job, but if you look closely you can see orange peel in the finish. Where as what I've been aiming at for several year is similar to the Custom Car show that makes my mouth drop because of the paint jobs, flawless and such deep looking finish + the details and I also see so much work and effort in getting these finishes.

In no way am I faulting the way other folks finish their products. Nor, am I boasting about my finishing, I'm not that great compared to the finishing galoots. But, I felt like I needed to respond to Fred and Clint's post, maybe we are speaking of a different grade of apples here(?). Just can not see going from raw lacquer on the wood to rubbing compound, seems like the wood bonnet wood round over the lacquer particles vs. being flattened by sanding.

Respectfully,

Dale

Re: My lacquer finishing process

#7

Re: My lacquer finishing process

Steve Jenkins, McKinney, TX.

>Dale, you might be spraying the coats too thin. The fact that you are shooting 4 coats and still sanding through gives me that feeling. The next time you are in Sherwin Williams ask them for a "mil gauge" so you can measure the thickness of your wet film when you spray.Usually they are given free or for a very nominal charge. Typically 3-5 wet mils is the "norm" for most finishes although it will say on the can.

Whether or not you use a "sealer" is your choice but not always necessary. An instance where it is needed I discovered the hard way. I was using M.L. Campbell Magnalac which is a precat and finishing a table top that I had stained and glazed. A couple months after finishing the finish was cracking. I called M.L. Campbell and was told that I needed to use a vinyl sealer over the glaze. Bingo no more problems. Of course I refinished the table three times before making the phone call.

anyway back to the finish.

get the mil gauge and try boxing the finish when you spray. In other words spray the whole surface in one direction ,say left to right, then immediately spray again the whole surface in a 90 degree direction. each coat should be around 2 mils. After that you should be able to sand with 320 or finer without going through the finish.

the answer to your question is a definite maybe. Today you may be able to skip the last step and go directly to polishing and tomorrow you may burn through. You have to remember that even though you are polishing you are still removing a tiny bit of the film.

Take some time and some scrap wood and try different things to see what works best for the final look you are after. I know I hate to finsh scrap too but it usually pays off at some point.

Steve

Re: My lacquer finishing process

#8

Re: My lacquer finishing process

Fred Davis

>Dale,

sounds to me like your trying for a French Polish finish which is a whole other system. You think your doing a lot of rubbing now , try French Polish.

I do not use a power buffer, old fashined I guess, but slick is slick, free of orange peel, runs, sags , pimples, dimples , all of which is indicative of improper application.

Go to a library and look up a book on finishing by George Frank, you will be glad you did.

FredD

Re: My lacquer finishing process

#9

Dale Lenz

Re: Thanks Fred,...

Dale Lenz

>purchased Franks book about 20 years ago, little green paperback if I recall correctly, but than again might be thinking of Planecraft, : ' >. Prior to sanding down the finial coats, lacquer appeared to be glass smooth, looked at the cherry's surface with a raking light and the workbench's light bulb was blurry. After sanding and compounding I could read the wattage and voltage off the light bulb at 35 inches, once again using a raking light. Got a mirror out and did the same thing, 35 inches was about as far as my eyes could read the light bulb verbiage. Pointed the mirror toward the ceiling, could of seen a fly on my tube lights some 5 feet higher, can't see that clearly on my cherry work, still need to practice more, : ' >. Books has scared me away from trying French polishing, TOO MUCH WORK! : ' >.

Happy 4th, 5th and 6th, : ' >.

Re: My lacquer finishing process

#10

Dale Lenz

Re: Thanks, Steve

Dale Lenz

>Will go the SW and ask for a mil gauge, hope they know what I'm talking about. Have not been impressed with our local SW folks. They don't know what I'm talking about half the time and I don't think it me, simple question for a finishing store, I think. Our SW store does not carry sandpaper past 400 grit. Went in the SW a year ago to purchase some wood filler, going to fill some oak grain prior to going after the high sheen, they tried to sell me that acetone putty stuff in the small plastic jars. Me think not many folks do the kind of finish I'm attempting to get around here.

One thing I've learn about sanding through on my finishing is not waiting 3 days or so for the lacquer to cure. I've burned through with rubbing compounds a few times, once again not wait for the lacquer to cure at least 3 days. I usually start off with Maguires med. stuff, #2(?), then go to #9, swirl remover and call it good. Once again thanks for all of you folks help and suggestions.