problems with a tung oil finish

Glenn

>I have an oak table that has been finished with tung oil many times over the years. When I moved to the new house the table now is in the sun for periods during the day. The tung oil is drawn out the pores in the wood towards the sun leave a sticky mess on the edge of the table. One solution I was considering is an oil based polyurethane to try to seal the pores. Any suggestions??

Re: problems with a tung oil finish

#2

Re: problems with a tung oil finish

Mike Schwing from Md.

>Shellac would be my choice of sealer for this. You could then topcoat with whatever you desire. Refinishing might not be the easiest thing from there, but the shellac will keep the pores from oozing.

I'm not one of the finishing experts here and look forward to reading their suggestions.

Re: problems with a tung oil finish

#3

Re: problems with a tung oil finish

Howard Acheson

>Let's back up a moment and look at what you have. What do you mean by "tung oil"? Is it real, 100% tung oil or one of the faux "Tung Oil Finishes"? What exactly did you apply?

I want to understand what's on the table before we can discuss possible remedies. Covering up an underlying problem will either not work or will be a short term solution.

I have never run into an oak table that can not be made as "good as new" or maybe even better than new.

Re: problems with a tung oil finish

#4

Re: problems with a tung oil finish

Glenn

>Howard: 100 % pure tung oil from Lee Valley was being used. The literature stated that it was support to harden to a finish and it was fine until the table was out in the sunlight

Re: problems with a tung oil finish

#5

Re: problems with a tung oil finish

Clint Searl, at the base of Haycock Mtn

>Whatever the underlying finish is, if left in the sun, it will continue to cook out, regardless of anything put on over top. The surist fix is to remove it completely with a MEC based stripper, wash it down with acetone, and refinish with shellac. I think well dried shellac is the least likely film finish to go south under the heat of the sun.

Clint

Re: problems with a tung oil finish

#6

Re: problems with a tung oil finish

Howard Acheson

>Contrary to whatever Lee Valley says, pure tung oil only "dries" to a certain extent. It really polymerizes as it reacts with oxygen for a semi-hard material. It never gets really hard.

What is probably happening is that the sun is heating up the surface and causing the tung oil to soften and even liquify in the pores. As it liquifies, it sort of bubbles up softening the top surface. After a number of years, you have a excessive build up of gunky oil.

I have two suggestions. First you an try to rub down the table using 3/0 steel wool and mineral spirits. Rub aggressively in the direction of the grain. Wipe off the gunk using lots of paper towels. Do it again. Then let if fully dry and see how it looks and feels. If it looks evenly use 4/0 steel wool and rub on a coat of thinned tung oil. Wipe the surface dry after letting it set for 15 minutes. Pure tung oil is very slow drying so leave it alone for at least a week. Instead of the tung oil, you could apply an oil/varnish mixture which would be more protective and more durable.

The second option--and the one I would do if it is a nice table--is to completely strip off the old finish. Use a chemical stripper containing methylene chloride. It will work the fasting and do the best job. This will get all the old oil off and present you with an almost virgin surface. Sand the surface smooth and then decide what type of finish you want. Again, I would not choose a pure oil as stated above. At the minimum, I would use an oil/varnish which will give you the same look and feel of tung oil but will be much more durable, protective and easy to maintain.

Re: problems with a tung oil finish

#7

No, no, no.

Michael Dresdner

>Strip it. Period. That is the quickest and surest way to get that uncured oil out of the pores. Refinish with varnish or polyurethane applied in thin coats.

As for this comment:

"I think well dried shellac is the least likely film finish to go south under the heat of the sun."

That is entirely incorrect. Shellac will soften at very low temperatures, and even cured shellac can bubble in direct hot sunlight, which is one reason we don't use it outdoors. The best heat resistance for common, single pack finishes comes with oil based polyurethane, and that is what I would suggest you use.