William

>need a little advice on finishing my pool table,Ive recently re-vennered a 90 year old pool table with mahogany. veneer was sanded to 220 and stained with red mahogany veneer.

What Ive done with one of the legs;

brushed on sanding sealer sanded with 400 grit and brushed on a second, sanded one more time with 400 then filled pores with behlens. let pores dry overnight and lightly sanded with 400 before top coating with deft clear spray lacquer.

I'm thinking after reading more and more that I should have used 220 in some of the steps and let the pore filler stand for a few more days

also some of the pores are still there can I sand the existing leg with 220 and fill it again? any help would be greatly appreciated

Bill

Re: Finishing

#2

Re: Yes/Depends *LINK*

Mark Mandell - Gone Round In Jersey

>You can treat the Deft as a sanding sealer (which it mostly resembles), cut it back (try 320) and reapply your filler. You can save yourself some work on the filler by gently rubbing cross grain with a piece of burlap to remove the excess. Overnight should be fine for allowing the filler to dry completely.

If your table is 90 years old, chances are the original finish is shellac. All you need do to restore an old shellac finish is to scrub it down with alcohol and a stiff brush, then wipe with a rag wet with alcohol and let dry. Refinish with dewaxed shellac (prefer a darker shade like Garnet or Dark Garnet on mahogony). I refinished a neighbor's mahogony game table this way and the piece simply bloomed.

As far as a final finish, you could do a lot better than Deft; especially in the solvent lacquer arena. Since I don't use the stuff anymore, I'll leave it to others to point you to a good brand. Since I will assume you'll want maximum durability on the rails and side-work, you should consider one of the acrylic waterborne lacquers or polys that can be cross-linked to give an even harder more durable finish. General's Super Poly or Enduro with cross-linker added come to mind, but there are others just as good or better depending on how much you want to spend [google "Unaxol"). Also suggest you log on to Jeff Jewitt's site at the link and post some questions on one or several of his finishing forums.


Homestead

Re: Finishing

#3

Re: Yes/Depends

William

>thank you, actually the table was re-veneered with mahgany so the finish is bare wood. Ive had a lot of luck with the Deft spray cans, the atomization is almost as good as a gun.

in case I didn't make it clear, I'm using deft sanding sealer and deft high gloss spray lacquer

Re: Finishing

#4

Re: Finishing

Steve Schoene

>First a few questions. What, specifically, was the red mahogany stain?

Which Behlen's pore filler did you use, the oil based or the water based?

If I understand, you have finished one leg, with the schedule:

sanding sealer 1 coat,

sanding sealer 1 coat

pore filler, excess removed from surface, lightly sanded and overnight cure.

lacquer 1 coat?

The other three legs have not had any finish applied?

Re: Finishing

#5

Re: Finishing

William

>the stain was minwax, red mahagany, I used Behlen's pore o pac "red mahagany" for the pore filler

Re: Finishing

#6

Re: Finishing

Steve Schoene

>I think I'd recommend a drastic step of stripping the one leg you have finished and starting over. That's the only way I think to get all the legs to end up the same, without the risk of problems down the road from the pore filler. Pore filler, covered before it has cured can, months later, can develop a white or greyish cast in the pores.

Use a stripper, not sanding, since with veneer you have precious little room for sanding. You may not get every trace of the stain out but probably enough. Follow the directions with the stripper completely. Then very lightly sand and stain the bare wood again.

I'd then put on one coat of 1 1/2 or 2 pound cut shellac to seal the stain and then apply the pore filler tinted to match, or be a bit darker than the stain, wiping off excess as it sets up. Then I'd give this at least 3-4 days to get well cured--I usually wait a week. Then after a very light sanding to remove any haze on the surface, you can apply the top coat that you want.

No sanding sealer is needed in this schedule. I don't see much point in it except for a few finishes, mostly catalyzed, where the finish manufacturer requires a specific sealer for that finish.

And, the general moral of the story is to always make a finish sample--using the same materials and preparation and carrying it all the way to the final finish. Let that be the place where you discover that you didn't like something you did.