Home Articles Forums Gallery Marketplace Videos

WoodCentral Forums

Knowledge You Can Build On — Est. 1998

Reach the woodworkers who ACTUALLY BUY

Shellac (again) What would happen if...

Posts

Shellac (again) What would happen if...

#1

Shellac (again) What would happen if...

Barry Irby

>I have posted over and over about my struggles with shellacing the top of my huntboard. Its better now, but not good enough.

Could somebody describe "rubbing out" to me? How do I achieve a nice low gloss surface?

And what would happen if you sanded it nice an smooth (but dull) and misted it with alcohol form a spray bottle? Would that slightly melt the surface and restore a nice level sheen?

Re: Shellac (again) What would happen if...

#2

Re: Shellac (again) What would happen if...

Dave Bair, Eaton Rapids, MI

>I'll let another explain rubbing-out. But I have tried the alcohol-on-top trick, both misting and brushing; they were both failures. One left heavy brush marks, the other left a multitude of pits (like orange-peel pores). You are never going to get a sheen (as opposed to shine) on shellac by using another layer of shellac. You have to treat the surface (rubbing-out), either by sanding and polishing or sanding and waxing.

Re: Shellac (again) What would happen if...

#3

Re: Shellac (again) What would happen if...

ted Wong

>I've had the best results with a very thinned out shellac mix made straigt from flakes.

It's way thinner than a typical 1 Lb. or 2 Lb cut and many applications I get a perfect finish.

I apply with a section of old T-shirt and wait two or more ours between applications. It's time consuming but I've never had a bad experience with this method.

Re: Shellac (again) What would happen if...

#4

Re: OK... Rubbing it out...

Glenn Madsen near San Francisco

>There are a number of ways to do this, and many here are more experienced than I. But here goes.

Take that clean lint free old tshirt you've been hanging on to since the sixties. And a squeeze bottle of the SealCoat you've been using, now cut 1 to 1 with denatured alcohol, or something fancier. Squeeze enough of the mix into the wiping pad to get it moist, but not wet. Just 'lay' a thin coat of shellac on, essentially touching once, and moving on. Like the French poishing wizards, you want to touch down easily, touch it barely, and lift the pad off easily. Cover everything once, then put the pad in ziplock bag, and go watch the golf match for four hours. Or three days.

Anyhow, let the shellac cure hard, not just evaporate the alcohol. Find yourself some of the 3M white 0000 extrafine synthetic steel wool. Not real steel wool, but the synthetic. Get yourself some soft furniture wax, in clear, like a Liberon Black Bison, or Briwax. Gently rub the piece with the pad, dipped in the wax, with the grain pattern. You're trying to cut the sheen of the shellac just enough to make it look like you want it to. Try very hard not to work cross grain, if you can help it. You want an even, very mild scratch pattern.

Then take an old, soft bath towel, and rub the piece well, after the wax dries, and bring up the soft shine. The more care you take, the better it looks. The bigger the surface, the more care you need to take. Rub it with the towel, turning the towel a lot to keep clean surfaces to take much of the wax off the surface.

Let it sit for a week, then wax it again, with the old towel this time. Buff it out again. Invite guests over for Sunday dinner to show off your new piece of artwork. Bask in the glow of well earned glory.

Re: Shellac (again) What would happen if...

#5

Re: Shellac (again) What would happen if...

Steve Schoene

>I begin the rubbing out process with 400 grit wet/dry sandpaper if there are any defects to remove. If the surface is smooth but you want to change the sheen you can start with a higher grit--say 600 or 800. You can lubricate with mineral spirits but but using it dry helps you see what is going on. Use the sandpaper on a lightly padded block to level out any defects. Steel wool (real or synthetic) follows contours and therefore doesn't level very well.

Once you have the surface level and evenly dull from the initial sanding, you can work to a finer grit, say to about 1200 or 1500 in a couple of stages. Where you go from there depends on what sheen you want. I use fine pumice, lubricated with paraffin oil (very light mineral oil) for a satin finish. If I want gloss I use rottenstone. More modern folks use rubbing compounds.

The step up in quality you get when you rub out the finish is large, with potential to make factory finished furniture look shabby.

Re: Shellac (again) What would happen if...

#6

Pumice/Rottenstone

Mike Fitterling

>I like to rub out shellac and lacquer the old fashined way; with a hard felt pad and pumice and rottenstone powder with oil as a lubricant (I use parafin oil). Just sprinkle a little powder on the piece and add some oil and start rubbing with the felt pad. Using pumice first will give a matte to satin sheen (depending on the grade of pumice) and moving on to rottenstone will give a glass-like gloss. You will need a different felt pad for each grit of powder. It also is a good idea to have numerous coats of the finish on before rubbing out.

Good luck,

Mike

Re: Shellac (again) What would happen if...

#7

Re: Pumice/Rottenstone

Barry Irby

>Mike, I have a top that is about 20" by 54". How long would you expect to spend on each "grit"? I bought Behlens 2F and 4F pumice and rottenstone, paraffin oil and pads.

I know this is a "How high is up" question with lots of variables but would you be looking at ten minutes per grit, an hour, two hours? Just a ball park.

Thanks.

Re: Shellac (again) What would happen if...

#8

rubbing out, quick and easy *LINK*

Michael Dresdner

>Here's a complete set of instructions direct from my website


Rubbing out a finish