how long to steam 1/16 thick for bending?
Bill Tindal, E.TN
>
Knowledge You Can Build On — Est. 1998
how long to steam 1/16 thick for bending?
Bill Tindal, E.TN
>
Re: Doesn't it bend without steaming??
JL
>I have hot water bent 1/16" wood (cherry and maple). I haven't steam bent it. I usually go for 45-60 minutes for 7/8" - 1" thick. I have bent 1/4" and 1/2" after 30 minutes and it worked fine.
Re: try hot pipe bending.
Ted Wong
>
Re: how long to steam 1/16 thick for bending?
Bruce, a MN Galoot
>seems to me the last time I made shaker boxes (maple and cherry sides) I soaked the sides in hot water for maybe 15 minutes and they bent fine.
If you're going to laminate the strips, then the time would be significantly less.
bruce
please explain or reference
Bill Tindal, E.TN
>
Re: how long to steam 1/16 thick for bending?
Sgian Dubh
>Typically you need about fifty minutes to an hour per inch of thickness Bill. This means getting the wood up to temperature all through and keeping it hot for sufficient time to become flexible. The following notes refer specifically to wood 1" (25 mm) thick and classic bending woods, e.g., white oaks, beech and ash.
The easiest to heat and steam is green wood-- it takes a bit less than an hour and it's already flexible because it's wet anyway and the fibres are soft.
Most people choose air dried wood as the best compromise at about 20- 25% MC. This stuff takes about an hour. You might be able to air dry to lower MC levels in your area, but here in the UK 20% MC is about as low as you'll ever get air dried stuff.
The least cooperative choice is kiln dried wood. And the least cooperative choice of all are generally American kilned wood species because it's dried to as low as 6% MC. This makes the whole heating and lignin and fibre softening process more difficult. I've seen kilned american white oaks take two hours of steaming to get them bendable, and results even then tend to be patchy.
So something air dried, about 1/16" thick, in a white oak will bend easily after about four or five minutes held at the raised temperature. Walnut is not bad for bending and cherry is not really a good choice, but both will bend if the grain is right and enough patience goes into the steaming process. It's possible to oversteam to the point that the fibres start to disintegrate and strength diminishes the more you steam.
Riven material bends the most successfully as the grain is uninterrupted for the length of the plank, i.e., the grain doesn't run out on the face due to milling/conversion operations at the sawmill.
A riven 1" thick oak plank is reckoned to have the same strength as a 2" thick sawn board because of the continuous grain. The Vikings proved this back before the year 1000 with their seafaring long ships which sailed all the way to Florida and back.
No handy references to point you at I'm afraid. This is all just stuff I've learnt over the decades from experience and all sorts of diverse written snippets here and there. Slainte.
Sorry, brain fart there.
Sgian Dubh
>Air dried timber in the UK will normally dry to about 18- 20% MC, but often higher by a point or two, and sometimes just a point or two lower. Sorry about that. Slainte.
Re: please explain or reference
Keith Newton
>Bill, the typical method of steaming only works if you can keep the temperature above 205� long enough to get the wood bent around the form after you remove it from the chamber. The problem when the wood it this thin, is that it can cool down faster than you can work. If you don't have enough heat, the cells don't slip past their neighbors to take a new memory, so it will tend to spring-back.
By supplying the heat with a pipe, you overcome that problem.
Here is a link that I found by goggling, luthier supplies, hot pipe.
http://www.diynetwork.com/diy/hb_musical_instruments/article/0,2033,DIY_13881_2857278,00.html
Well, that explains my failures
Bill Tindal, E.TN
>