Time to clear things up
Michael Dresdner
>First, Jasper is exactly right. Driers speed up some (not all) drying oils, but have no effect whatever on non-drying oils such as mineral oil.
There are many different driers and they work differently. Some are top or skin driers, some are through driers. Some oils are very much affected by them, some are not, and some respond only to certain ones, or only in a limited way.
The MSDS cited in the posted link is cobalt drier, which is one of the through driers. Other common driers besides cobalt include zinc, lead, manganese, magnesium, and selenium, though there are others. As a group they are metal salts or metal naphthanates.
If you add driers to a drying oil like linseed oil, they speed up the oxygen polymerization. Because they are true catalysts, they do not become part of the final molecule. However, in the course of going from liquid to solid, the finish forms a matrix in which is trapped the metal salts. In other words, once the finish cures, it is quite unlikely that the metals will migrate out unless affected by a chelating compound.
The bottom line is that while consuming large amounts of these metals is harmful, the odds of doing that from a cured finish is slim indeed.
You have probably already noticed that we humans do regularly consume small amounts of many of these metals, and some, like zinc and selenium, are crucial to good health. It is all about amount.
One word of warning: adding too much drier can have the opposite effect, preventing the finish from curing. What is too much? That depends on which drier you are using, what you are adding it to, and how much of what type of drier is already in the mix. Some driers have a synergistic effect on one another, meaning much smaller amounts in combination can have far more significant results. For this reason I alway caution people about adding driers to finish in a cavalier manner.